Several years ago I completed some tests on removing silicon oil from
aluminum plates. I experimented with Freon, MEK, several different citrus
and pine based solvents, and a detergent and water (Cascade dishwashing
detergent in a dish washer). I then primed one half of the plate with metal
primer and left the other half bare. A .250 layer of a urethane potting
material was bonded to the plates and cured. Peel tests were performed and
the highest strength peel came from the plate cleaned in Cascade in a
dishwasher. You might want to try it yourself.
Jan Satterfield
Sr. Mfg Engineer
L-3 Communications
> -----Original Message-----
> From: Jim Marsico 516-595-5879 [SMTP:[log in to unmask]]
> Sent: Thursday, August 12, 1999 6:23 AM
> To: [log in to unmask]
> Subject: [TN] SILICONE CONTAMINATION
>
> Good Morning Technet:
>
> Can anyone suggest methods of cleaning cast aluminum plates of silicone
> residue (from a silicone-based machining oil)? These plates must be clean
> enough to bond to using a structural epoxy.
>
> Thanks...
>
> Jim Marsico
> AIL Systems Inc.
> (516) 595-5879
> [log in to unmask]
>
>
> ##############################################################
> TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
> ##############################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with
> following text in
> the body:
> To subscribe: SUBSCRIBE TECHNET <your full name>
> To unsubscribe: SIGNOFF TECHNET
> ##############################################################
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> additional
> information.
> If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
> 847-509-9700 ext.5365
> ##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
|
|
|