Ed Cosper wrote:
>
> Has anyone ever experienced a problem of copper sulfate crystals developing on the bottom of anodes inside the anode bags? If so, what causes it and how do you get rid of it.
>
> thanks,
>
> Ed Cosper
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
> To subscribe: SUBSCRIBE TechNet <your full name>
> To unsubscribe: SIGNOFF TechNet
> ################################################################
> Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
> For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311
> ################################################################
Generally this is caused by inadequate exchange of solution in the anode
bag with bulk solution. The weave of the anode bag is either too tight
or has become plugged. Interior solution continues to build in CuSO4
concentration due to anode disolution until the interior solution
becomes super saturated and crystallization is inevitable. Either clean
andode bags or reduce the nap and weave in future anode bags.
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311
################################################################
|
|
|