TECHNET Archives

August 2000

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-type:
text/plain; charset=us-ascii
Sender:
Subject:
From:
David Hillman <[log in to unmask]>
Date:
Wed, 16 Aug 2000 08:48:22 -0500
MIME-Version:
1.0
X-To:
Milanie Racuya <[log in to unmask]>
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, [log in to unmask]
Parts/Attachments:
text/plain (74 lines)
Hi Bing! Test the solderability of the problem capacitors using
specification ANSIJ-STD-002A to see if the solderability of the end
terminations is an issue. Good Luck.

Dave Hillman
Rockwell Collins
[log in to unmask]





Milanie Racuya <[log in to unmask]>@IPC.ORG> on 08/16/2000 08:14:40 AM

Please respond to "TechNet E-Mail Forum." <[log in to unmask]>; Please respond
      to Milanie Racuya <[log in to unmask]>

Sent by:  TechNet <[log in to unmask]>


To:   [log in to unmask]
cc:

Subject:  [TN] Unsoldered joint on chip capacitor


Hi guys,
Just want to ask advice on what else to do on the unsoldered joints we
are encountering regarding one vendor of the chip capacitor.
We were using other vendors at that time then we used this one and it
caused us a lot of headache. Same SMT machine settings, same solder
paste, same ambient temperature and humidity. But using the new
capacitor with the said vendor, we already had a problem on unsoldered
joint.
     Does this mean that the solder paste we are using is not compatible
with the component termination???
     What we are doing right now is to drop a small amount of flux on
the affected locations before processing it in the reflow.
     What advice can you still give me??? We are doing all what we can
and yet, still the occurrence of unsoldered joints.

Regards,
Bing

##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in
the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################

##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################

ATOM RSS1 RSS2