TECHNET Archives

March 1998

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
Subject:
From:
Padmanabha Anandapuram Halappa <[log in to unmask]>
Date:
Tue, 10 Mar 1998 19:57:14 EST
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, [log in to unmask]
Parts/Attachments:
text/plain (96 lines)
This is a MIME-encapsulated message

--GAA19645.889530115/www2.viasystems.com

The original message was received at Tue, 10 Mar 1998 06:41:52 -0500 (EST)
from venus.likom.com.my [192.228.164.33]

   ----- The following addresses had permanent fatal errors -----
<charles,[log in to unmask]>

   ----- Transcript of session follows -----
... while talking to mailer2.viasystems.com.:
>>> RCPT To:<charles,[log in to unmask]>
<<< 553 malformed address: <charles,[log in to unmask]>
550 <charles,[log in to unmask]>... User unknown

--GAA19645.889530115/www2.viasystems.com
Content-Type: message/delivery-status

Reporting-MTA: dns; www2.viasystems.com
Received-From-MTA: DNS; venus.likom.com.my
Arrival-Date: Tue, 10 Mar 1998 06:41:52 -0500 (EST)

Final-Recipient: RFC822; charles,[log in to unmask]
Action: failed
Status: 5.1.1
Remote-MTA: DNS; mailer2.viasystems.com
Diagnostic-Code: SMTP; 553 malformed address: <charles,[log in to unmask]>
Last-Attempt-Date: Tue, 10 Mar 1998 06:41:54 -0500 (EST)

--GAA19645.889530115/www2.viasystems.com
Content-Type: message/rfc822

Return-Path: <[log in to unmask]>
Received: from venus (venus.likom.com.my [192.228.164.33])
 by www2.viasystems.com (8.8.6/8.8.6) with SMTP id GAA19643
 for <charles,[log in to unmask]>; Tue, 10 Mar 1998 06:41:52 -0500 (EST)
From: [log in to unmask]
Received: from smtpgwy.likom.com.my by venus (5.x/SMI-SVR4)
 id AA01921; Tue, 10 Mar 1998 19:52:26 +0800
Received: from cc:Mail by smtpgwy.likom.com.my
 id AA889588194; Tue, 10 Mar 98 19:48:55 EST
Date: Tue, 10 Mar 98 19:48:55 EST
Encoding: 32 Text
Message-Id: <[log in to unmask]>
To: "charles''"<charles>, [log in to unmask]
Subject: Grainy copper deposit.

     dear Mr.charles,
     thank you for the reply,following are the information regarding
     plating process.
      additive ...copper gleam 125 T,LEA RONAL.4-5 ML/LTR
                   suggestion 7.5-10 ml/l
     copper sulfate...75-85g/l
     sulfuricacid...100-110ml/l
     chloride...50-60ppm.
     this problem started when we attempt to raise additive content
     from 5ml/l to 7.5ml/l.this problem appeared,one week after the
     addition of extra brightener.7.5 ltr brightener added at a time
     to 4 copper tanks of 3000 ltr each.(7.5ltr/tank.).
     IN the beginning we suspeccted organic contamination,& anode sludge.
     carbon treatment done,anode baskets cleaned.
     again we try maintain additive at 7.5ml/l as per vendor suggestion.
     cvs used to analyse addditive content.
     after one week GRAINY COPPER reappeared on the panels,since hard
     deburring did not help & have to scrap beacause of cosmetic.
     Since 125 T is one component (pre mixed leveller,brightener,&carrier)
     vendor did not help on analysing it seperatly.
     This grainy copper repeated atlest 5 times,eventhough sometime no
     addition (additive) made.
     since vendor did not help much on this ,I used stop addition of
     brightener ,atlest 2 shift,to stop this problem.vendor reply is
     our predip acid copper is high.
     this grainy copper most of the time on highcurrent area.
     The current density in use 1.5 to 2.1
     the panels with 1.8to 2.1 ASD normally get this problem.
     anode balls of 1" dia are being used.
     thanks & expecting a Positive reply to understand 125T.
     padmanabha.A,H.



--GAA19645.889530115/www2.viasystems.com--

################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe:   SUBSCRIBE TechNet <your full name>
To unsubscribe:   SIGNOFF TechNet 
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311
################################################################


ATOM RSS1 RSS2