TECHNET Archives

June 2002

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
Subject:
From:
Bev Christian <[log in to unmask]>
Date:
Fri, 21 Jun 2002 09:07:04 -0400
Content-Type:
text/plain; charset="iso-8859-1"
MIME-Version:
1.0
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, Bev Christian <[log in to unmask]>
Parts/Attachments:
text/plain (79 lines)
OK, now the games begin!  :)  We have two replies so far to my question
:"How big of a crack in thermally cycled solder
joints is too big of a crack?"

Werner, I am a little confused by your statement "I also assume he does not
include in "if you can detect it, it is too big!" cross-sectioning."
Could you please elaborate?

I was NOT trying to make a technical connection between BGA voiding and this
issue.  I was trying to draw a parallel between the possible arguments of
what is the max largest % voiding and possible arguments about crack size.
Sorry if I confused people!

So, Werner, when does a micro-crack become a crack, in terms of size?

regards,
Bev Christian
Research in Motion

-----Original Message-----
From: Werner Engelmaier [mailto:[log in to unmask]]
Sent: June 21, 2002 7:24 AM
To: [log in to unmask]
Subject: Re: [TN] cracks in solder joints


Hi Bev, David & All T's,
While I concur with David's "big enough" statement, I also assume he does
not
include in "if you can detect it, it is too big!" cross-sectioning.
On the other hand, Bev writes "Shades of voids in BGAs...   How big of a
crack in thermally cycled solder joints is too big of a crack?"
Cracks in thermally cycled solder joints have nothing to do with voids;
therefore why "Shades of voids in BGAs...". Solder exhibits micro-voids
[having nothing to do with voids] at grain boundary intersections after
about
25 to 30% of the fatigue life having been consumed, and micro-cracks along
grain boundaries after about 40%. That means about 60% of life is still
available when 'observable' micro-cracks are present.
David then says: "A better question would be how do you distinguish between
a
crack and a void?"
That one is easy, voids a roughly spherical, cracks are fractures.

Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL  32174  USA
Phone: 386-437-8747, Fax: 386-437-8737
E-mail: [log in to unmask], Website: www.engelmaier.com

----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

ATOM RSS1 RSS2