TECHNET Archives

April 2009

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Steve Gregory <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Steve Gregory <[log in to unmask]>
Date:
Thu, 23 Apr 2009 13:42:54 -0500
Content-Type:
text/plain
Parts/Attachments:
text/plain (56 lines)
Hi John,

Yeah, like I said when I sent you the links to your pictures, the last time we had a bad solderball problem we got a bad lot of paste, and to our vendors credit, they admitted the paste was bad. 

But I went back and looked at the picture of the solderball problem we had (I learned a new term then, "snotballs", which was what our vendor called it), and it doesn't look anything like your problem. Check out:

http://stevezeva.homestead.com/files/Snotballs.jpg

I have a question; do all of the boards during a run look like the pictures, or do you get a few boards out of the run that look okay?

Steve

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of John Parsons
Sent: Thursday, April 23, 2009 1:16 PM
To: [log in to unmask]
Subject: [TN] Solder Ball Problem

I am trying to get to the root of a little solder ball problem.  The problem is specific to a single part and was evident on the first run of this board a few months ago.  We are seeing it again on this run although the common denominator here is that the PCB's are all from the same production batch.

It appears that the formation of solder balls can be reduced by pre-baking the PCB's (100°C for 4-8 hrs) but not eliminated.  The best results are obtained by pre-conditioning the PCB's by running them through the reflow oven first,  letting them cool, then print, populate and re-flow.  The majority of balls now formed are dealt with at wash.

The PCB's are simple double sided, HASL finish.  I suspect a problem with the solder finish (HASL) but what exactly that "problem" is I am not sure.
FYI, paste is water soluble.

http://stevezeva.homestead.com/files/Solder_ball_1.jpg - this photo is of a board that was pre-baked for about 4 hours @ 100°C, it was then printed and re-flowed.  It does not matter if the 4 hour bake improved things you can see that the results are pretty spectacular.

The following pictures are really more of the same except that these boards have been populated and washed. 

http://stevezeva.homestead.com/files/Solder_ball_2.jpg
 
http://stevezeva.homestead.com/files/Solder_ball_3.jpg
 
http://stevezeva.homestead.com/files/Solder_ball_4.jpg

Any insight would be appreciated.

(thanks to Steve for hosting the photos)

Regards
John Parsons

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2