Hi Jorge! There a number of books (Lau, Clech, etc) that can give you more
detailed issues on why LCCs can be a problematic component style. The CTE
mismatch between the LCC (a ceramic, CTE around 6ppm) and the pwb laminate
(an organic, CTE around 17ppm) results in a fair mount of stress thus
damaging the solder connection. The LCC design compounds the stress issue
by using a lead configuration that is both the electrical and mechanical
component connection to the printed wiring assembly. Most high performance
electronics applications do not use LCC components. Other TechNet folks
will fill in several other LCC issues. I don't recommend using them on any
printed wiring assembly. Good Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
Jorge.Rodriguez@VA
RIANINC.COM To: [log in to unmask]
Sent by: TechNet cc:
<[log in to unmask]> Subject: [TN] LCC process and manufacturing recommendations
10/15/2004 12:52
PM
Please respond to
TechNet E-Mail
Forum; Please
respond to
Jorge.Rodriguez
Fellow technetters,
I taught of using Technet's pool of knowledge to get some recommendations
on
LCC type devices. We have a customer asking questions on this package, and
all I know is that there are concerns of solder joint cracking due to
board/ceramic CTE mismatch.
What are the pros and cons of LCC devices?
Process and manufacturing recommendations?
Solder joint reliability?
Reliability under extreme environment conditions?
Any comment would be greatly appreciated.
Thanks!
Jorge A Rodriguez
Sr. Process Engineer
Varian, Inc
480-968-6790 X 4258
[log in to unmask]
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|