No, the immersion gold in the ENIG process is a self-limiting deposit and
will be 3 - 8 microinches; the thickness of the plated gold in the
electrolytic process will be much harder to control; we spec 3 - 15
microinches (and sometimes get pushback). As Jeff said, it is the nature
of the beast for a electrolytic-plated process to have deposit variability
based on circuit density (and tank design; and anodes; etc and so forth).
"Flash" is normally used to mean a thin, sacrificial coating of *plated*
hard gold.
Valerie
John Parsons <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
04/19/2005 05:12 PM
Please respond to TechNet E-Mail Forum; Please respond to John Parsons
To: [log in to unmask]
cc:
Subject: Re: [TN] ENIG vs Flash Gold
Sure, understood. I should be able to hold them to similar Ni and Au
thickness specs as for ENIG no?
John Parsons
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Eddie Rocha
Sent: Tuesday, April 19, 2005 2:07 PM
To: [log in to unmask]
Subject: Re: [TN] ENIG vs Flash Gold
Flash gold is too general of a term. If you are to solder to the thinner
gold successfully it must be less than 20 uin.
-- Thanks,
Eddie Rocha
South Bay Circuits
(480) 940-3125 x122
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
-
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|