Dan,
Yes, many of the low residue fluxes can be successfully cleaned with the
right saponifier and batch wash parameters. I would suggest that you
contact Kyzen Corporation. They have done a great deal of work on
chemistries to clean low residue fluxes, in both in-line and batch
operations. They have looked at almost every flux made. We are a Kyzen
house here at Rockwell. They support their products very well.
Charlie Pitarys of Kyzen regularly hangs out on this forum. I suspect he
will be contacting you.
Doug Pauls
Rockwell Collins
Dan Mauro <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
03/05/2008 06:35 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Dan Mauro <[log in to unmask]>
To
[log in to unmask]
cc
Subject
[TN] Cleaning No-clean
Folks,
I have a need to clean No-clean residue from PCBA's. Can this be
achieved with water washer and some type of saponifier ? Can anybody
suggest a batch process?
Thanks,
Dan
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|