TECHNET Archives

June 2007

TechNet@IPC.ORG

Options: Use Proportional Font
Show HTML Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Vladimir Igoshev <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Vladimir Igoshev <[log in to unmask]>
Date:
Wed, 13 Jun 2007 14:39:58 -0400
Content-Type:
text/plain
Parts/Attachments:
text/plain (1 lines)
You probably are :-) , BUT Ni has nothing to do with BP



Vladimir



-----Original Message-----

From: TechNet

To: [log in to unmask]

Sent: Wed Jun 13 14:31:03 2007

Subject: Re: [TN] Nickel barrier and RF applications



And it precipitates, not participates. The only thing nickel

participates in is creating brittle-nickel syndrome and BP! Ain't I an

old fussy fluxxer! 



-----Original Message-----

From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D.

Sent: Wednesday, June 13, 2007 12:57 PM

To: [log in to unmask]

Subject: Re: [TN] Nickel barrier and RF applications



Inge and Vlad

Keep in mind that Paymon is reflowing the entire assembly, not just

reworking a BGA site.

Therefore what you just described is happening over the entire assembly

to all of the solder joints. 

This cumulative effect could theoretically create a noticeable

improvement in the RF performance of the circuitry. 



-----Original Message-----

From: Hfjord [mailto:[log in to unmask]]

Sent: Wednesday, June 13, 2007 12:13 PM

To: 'TechNet E-Mail Forum'; Stadem, Richard D.

Subject: SV: [TN] Nickel barrier and RF applications



For each repeated reflow, more and more nickel participates in building

nickel/tin intermetallics. These IMCs are not ferromagnetic. So, let's

assume that Paymon's electroless nickel is just some 2-3 micrometers

thick, which is not unusual, then a growth of the IMC by some 0.1 to 0.5

micrometer for each reflow will probably have a positive effect = less

magnetic. 

Just an analogue thought

Inge





I think, there is one question to ask. If ENIG (or rather the presence

of Ni) is the source of the problem, then why does 2nd reflow improves

the yield?





Regards,



Vladimir

AMD



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0 To

unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or

(re-start) delivery of Technet send e-mail to [log in to unmask]: SET

Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the

posts: send e-mail to [log in to unmask]: SET Technet Digest Search the

archives of previous posts at: http://listserv.ipc.org/archives Please

visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for

additional information, or contact Keach Sasamori at [log in to unmask] or

847-615-7100 ext.2815

-----------------------------------------------------



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815

-----------------------------------------------------






ATOM RSS1 RSS2