     How would pumice scrub play in the formation of nodules and what 
     preclean stage may you be referring to?
     
     Don Hoppe - Zycon


______________________________ Reply Separator _________________________________
Subject: Re: Copper plating
Author:  [log in to unmask] at corp
Date:    12/19/96 9:48 PM


I would suggest looking more closely at the preclean. Is it possible that 
you are using Aluminum oxide or pumice preclean?
     
Dave Rooke
Circo Craft - Pointe Claire
     
---------------------
>We have been exhibiting miniature size nodules on our panels for quite 
>some time. These miniatue nodules resemble a slightly high brightner 
>burn. 
>I was wondering if anybody can give me a few suggestions to where I 
>should look. 
> 
>Afew test I have ran were with bare laminate through a scrubber before 
>plating. Nodules appeared on them. 
> 
>Afew more experiments were ran through different preclean lines and all 
>led to the same result, nodules.
>
>My questions if anybody could help are:
>1. Would a rectifier with too high ripple affect the leveling of copper 
>plating?
>2. We currently hot load our racks into the bath, the program is set up 
>with a five second lag  and raises from 0 amp to calculated amperage. So 
>the panel sees 5 seconds of 0 amps before the rectifier applies voltage. 
>Could this be a contributor? 
>
>Timothy Gaylor
     
*************************************************************************** 
* TechNet mail list is provided as a service by IPC using SmartList v3.05 * 
*************************************************************************** 
* To unsubscribe from this list at any time, send a message to:           * 
* [log in to unmask] with <subject: unsubscribe> and no text.        * 
*************************************************************************** 
* If you are having a problem with the IPC TechNet forum please contact   * 
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask]      * 
***************************************************************************
     

***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To unsubscribe from this list at any time, send a message to:           *
* [log in to unmask] with <subject: unsubscribe> and no text.        *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact   *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask]      *
***************************************************************************



ATOM RSS1 RSS2