TECHNET Archives

September 2004

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Gabriela Bogdan <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Gabriela Bogdan <[log in to unmask]>
Date:
Fri, 10 Sep 2004 19:12:02 +0200
Content-Type:
text/plain
Parts/Attachments:
text/plain (110 lines)
Ramon, Bev, Dave,
Thank you very much.
The leads are tin plated. but I saw them only after soldering. I have to
check if I can get a new component from the same batch- but I can not be
sure that its leadframe will be from the same batch.
But how will we know if we get such components?
Do a solderability test for each batch?
I suppose that the leadfree rush caught a lot of component suppliers
unprepared, and I doubt that they all do tests on the leadframes they order.
Gaby

----- Original Message -----
From: "David D. Hillman" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Friday, September 10, 2004 6:48 PM
Subject: Re: [TN] Tin plating on leads HELP!!!


> Hi Gaby! Do you know what the component lead surface finish is (what
> type/kind of plating)? Some plating types - like bright acid tin plating -
> could be the source of the solderballs.  And yes, the 002B surface mount
> simulation test would be helpful in determining root cause.
>
> Dave Hillman
> Rockwell Collins
> [log in to unmask]
>
>
>
>                       Gabriela Bogdan
>                       <gabriela@NETVISI        To:       [log in to unmask]
>                       ON.NET.IL>               cc:
>                       Sent by: TechNet         Subject:  [TN] Tin plating
on leads HELP!!!
>                       <[log in to unmask]>
>
>
>                       09/10/2004 11:24
>                       AM
>                       Please respond to
>                       TechNet E-Mail
>                       Forum; Please
>                       respond to
>                       Gabriela Bogdan
>
>
>
>
>
>
> Dear friends,
> After assembly, on all circuits there was one fine pitch PLCC from a
> certain vendor which had lots of small solder balls between the leads,
even
> on the solder mask dam between them.
> Other PLCC's with the same pitch were clean.
> We tried to see the amount of solder balls by X-ray, and found many more
> behind the leads.
> At first we thought that our solder paste was the culprit, but seeing that
> other components were "normal" , we looked closer to the leads by X-ray,
> and saw a lot of small voids only along the leads of the bad component,
> these voids reaching to the upper end of the leads, where the solder paste
> did  not reach. Visually, the upper part of the leads was very rough.
> I suppose that the tin plating of the leads contained additives which
epand
> during soldering, even burst out, and "spit" the molten solder all around.
> If this is the case,how could I reject such components during incoming
> inspection?
> Should I do a solderability test for each batch on a printed ceramic
plate?
> Gaby
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> -----------------------------------------------------
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
> -----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2