Hi Werner
Many thanks for an insightful answer.
Might it be possible to gain an increased thickness of solder between a chip components metallization and the PCB by designing
with a pad that matches the underside metallisation and having a stencil aperture that is larger than the PCB pad (perhaps not
larger at the 'toe' for tombstoning reasons).
Best Regards
David Greig
_____
From: [log in to unmask] [mailto:[log in to unmask]]
Sent: 19 October 2006 13:07
To: [log in to unmask]; [log in to unmask]; [log in to unmask]
Subject: Re: [TN] Tombstoning and nitrogen
Hi David,
What happens with all chip components and large pads is, that most of the solder goes for the fillets and very little winds up
between the chip and the PCB pad. Thus, the stand-off height, one of the prime reliability parameters, is very small and you get
crack initiation underneath the chip very early. What the fillets do in this case is provide functional life because of the
larger volume through which the cracks need to propagate for functional failure. Out in the fillets the cyclic strains are
smaller than underneath the chip, because of a much larger 'effective' solder joint thickness.
However, you would be much better of if the solder were underneath the chip instead of the in the fillet, thus preventing any
premature crack initiation in the first place.
Werner
--
Virus scanned by Lumison.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|