David,
You can do this if you are using a water soluble paste and wash the
assembly. You should not consider doing it if you are using a no-clean
process. The reason is that some paste invariably does not agglomerate
into the solder joint during the reflow process if it is not printed
onto the metal pad, but spatters leaving small solder balls. Even if you
use a water wash process it may still not be a good idea. Typically a
.006" or .007" thick deposit of paste is sufficient if the pad is the
same or almost the same size as the component endcap.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David Greig
Sent: Thursday, October 19, 2006 1:41 PM
To: [log in to unmask]
Subject: Re: [TN] Tombstoning and nitrogen
Hi Werner
Many thanks for an insightful answer.
Might it be possible to gain an increased thickness of solder between a
chip components metallization and the PCB by designing with a pad that
matches the underside metallisation and having a stencil aperture that
is larger than the PCB pad (perhaps not larger at the 'toe' for
tombstoning reasons).
Best Regards
David Greig
_____
From: [log in to unmask] [mailto:[log in to unmask]]
Sent: 19 October 2006 13:07
To: [log in to unmask]; [log in to unmask]; [log in to unmask]
Subject: Re: [TN] Tombstoning and nitrogen
Hi David,
What happens with all chip components and large pads is, that most of
the solder goes for the fillets and very little winds up between the
chip and the PCB pad. Thus, the stand-off height, one of the prime
reliability parameters, is very small and you get crack initiation
underneath the chip very early. What the fillets do in this case is
provide functional life because of the larger volume through which the
cracks need to propagate for functional failure. Out in the fillets the
cyclic strains are smaller than underneath the chip, because of a much
larger 'effective' solder joint thickness.
However, you would be much better of if the solder were underneath the
chip instead of the in the fillet, thus preventing any premature crack
initiation in the first place.
Werner
--
Virus scanned by Lumison.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|