Hi Brian,
A soldered contact is not designed for press-fitting (ie compliant
press-fit pin). You will not form a gas tight seal between the pin and
the hole/barrel wall even though the pin is tight. The pin might even
fracture the barrel causing an open or longer term intermittent/open. I
would not use your application for class 2 or class 3.
I have had no problem press-fitting a compliant press-fit pin (connector,
180 pin) in to a ENIG plated barrel/board. As long as you specifiy the
PTH tolerance recommended by the press-fit pin manufacturer.
Kerry
Kerry McMullen
Principal New Product Mfg. Engineer
LTX Corporation
825 University Avenue
Norwood, MA 02062-2643
(T) 781-467-5468
(C) 508-631-1832
(F) 781-461-0993
[log in to unmask]
Sent by: TechNet <[log in to unmask]>
09/12/2006 11:23 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
[log in to unmask]
To
[log in to unmask]
cc
Subject
[TN] Press Fitting Soldered Contacts Into ENIG
Good morning all,
Are there any particular reliability concerns when press-fitting a
soldered contact (SN63) into a plated barrel with an ENIG surface? What
might the outcome of this be over the long term? Is this an accepted
practice? Would this be acceptable in a class 3 military application?
Thank you for your input.
Brian Guidi
Senior Product Engineer
Teledyne Printed Circuit Technology
Tel: (603) 889-6191 X:310
Fax: (603) 886-2977
E-mail: [log in to unmask]
Visit us @ http://www.tetpct.com
Any technical information attached to this document is intended for the
recipient only. Also, the export and use of the information is regulated
by the export laws of the United States. Diversion contrary to U.S. law
is
prohibited. U.S. law prohibits sharing this information with any end-user
for any end-use related to the design, development, production,
stockpiling
or use of chemical, biological or nuclear weapons or missiles, without the
prior approval of the United States Government.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|