     Ralph
     
     Thanks for your inputs. I should have been more explicit. The laminate 
     voids are definately in the pre-preg. The usually around the pad on 
     the N-1 layer. Some have shown on other layers throughout the 
     stack-ups but primarily N-1. If we have laminate voids usually is 
     after solder float, some in as-built. Stack-ups vary on the board type 
     but the anamoly is random.
     
     We dessicate our prepreg in nitrogen cabinets prior to use but do not 
     vacuum evacuate. We have never had this problem.
     
     Thanks


______________________________ Reply Separator _________________________________
Subject: Re: FWD>Laminate Voids
Author:  [log in to unmask] at esdigate
Date:    5/24/96 11:51 AM


_____________________________ Reply Separator _________________________________ 
Subject: FWD>Laminate Voids
Author:  [log in to unmask] at SMTPpost1 
Date:    5/23/96 9:12 PM
     
     
Mail*Link(r) SMTP               FWD>Laminate Voids
     
<[log in to unmask]> inquired about "laminate voids" with the 
following:
     
>We are looking for some help with a processing anomaly which surfaced 
> ~ six months ago. We began to see laminate voids in our epoxy boards. 
>Polyimide does not seem to be affected. We have verified lamination 
>cycles, investigated layer clean, oxide thickness and pre-clean. 
>Solutions seem to remain random. We are running low on ideas. 
     
>Has anyone out there experienced the same problems? Solutions? Riston 
>residues? Conversion coatings?
     
>From: [log in to unmask]
     
You probably have volatiles absorbed (moisture or solvent(s)) in the base 
(core) material or in the prepreg.
     
If you have subsurface voids, in your cross sections you should be able to 
tell if the voids are in the core or prepreg
     
If the voids are in the core material, then it is a supplier problem.
     
If the voids are in the pregreg layers of the printed board then it can be 
either a core or prepreg material problem.  In both cases, volatilize-out the 
materials prior to lamination using some form of desiccation such as heat 
and/or vacuum.  
     
If the voids are surface and you are foil laminating, you most probably have 
volitles in the prepreg and need to desiccate as above.
     
Ralph Hersey