This is done by utilising the fact that copper oxide has a slightly lower
melting point than pure copper, so oxidised copper parts are run through a
furnace at just over the oxide melting point and below the metal melting to
"solder" the liquid copper oxide into the ceramic (usually aluminium oxide /
alumina). The process was originally developed by GE so you could try there,
or current suppliers like Kuramik in Germany, Toshiba and so on might be
able to help you.
Kind Regards
Mike Fenner
Applications Engineer, European Operations
Indium Corporation
T: + 44 1908 580 400
M: + 44 7810 526 317
F: + 44 1908 580 411
E: [log in to unmask]
W: www.indium.com
Leadfree: www.Pb-Free.com
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Dennis J. Fall
Sent: Thursday, June 06, 2002 7:54 PM
To: [log in to unmask]
Subject: [TN] Direct copper bonding
Where can I get more information on how to perform direct copper bonding to
alumina?
Thank You,
Dennis Fall
Process Engineering Supervisor
Thin Film Technology Corporation
North Mankato, MN 56003-1702
Email: [log in to unmask]
Phone: 507-625-8445
Fax: 507-386-9269
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|