TECHNET Archives

August 2004

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, R Sedlak <[log in to unmask]>
Date:
Wed, 11 Aug 2004 21:40:54 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Aleks Lozinsky <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
7bit
Content-Type:
text/plain; charset="iso-8859-1"
From:
Aleks Lozinsky <[log in to unmask]>
Parts/Attachments:
text/plain (86 lines)
Hi Dave,
You may wish to try wirebondable soft gold plating. It has higher
purity,different crystal structure, deposit properties. Hard gold much more
loaded with organics and metallic brighteners (Ni or Co) and normally better
suits for high wear resistance.
Aleks Lozinsky
Technic Toronto
----- Original Message -----
From: "R Sedlak" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Wednesday, August 11, 2004 8:50 PM
Subject: Re: [TN] SOFT Gold Plating/Contaminate Question


Dave:

The purpose of plating brighteners is to co-deposit, and muck up (a
technical term, meaning to "muck-up") the chrystalline deposit, and make it
shiney.  And if you get too many, or you get some brightener breakdown
problems, which does occur a lot in gold plating, because of the inert
anodes, you can get excessive organics in your gold.  And the type of
structures you are seeing are exactly what you would expect...

See, contrary to the common wisdom, electroplating does (sometimes) follow
the rules of chemistry.

Rudy Sedlak

"David D. Hillman" <[log in to unmask]> wrote:
Hi TechNet! Hey, looking for some help (Rudy, Frank, Gerard, plating
folks). Background: I have a test board which with approximately 80
uinches of wirebondable hard gold plating that is having gold wirebond
process problems. An XPS (xray photoelectron spectroscopy) analysis of a
"good" versus "bad" test board revealed that the "bad" has significant
organic surface contamination for carbon and oxygen in the form of a
hydrocarbon (lots of C-C and C-H bonds). Now the question: can/will a
hydrocarbon species be codeposited into the gold plating thickness? I
understand the surface process/issues but the codeposit question came up.

Dave Hillman
Rockwell Collins
[log in to unmask]

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------

__________________________________________________
Do You Yahoo!?
Tired of spam?  Yahoo! Mail has the best spam protection around

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
http://mail.yahoo.com

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2