TECHNET Archives

September 1999

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Type:
multipart/alternative; boundary="openmail-part-0b11ea98-00000002"
Sender:
Subject:
From:
Chris Evans <[log in to unmask]>
Date:
Wed, 29 Sep 1999 08:34:12 +0100
MIME-Version:
1.0
X-cc:
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, [log in to unmask]
Parts/Attachments:
BDY.RTF (352 bytes) , BDY.RTF (727 bytes)
Patty

Someone already mentioned "Modern Electroplating" by Lowenheim for
Platinum - it give a couple of pages on Indium plating as well.  

Example of typical solution
15 - 30 g/l In ( As fresh precipitate of hydroxide )
20 - 30 g/l D-glucose
140 - 160 g/l KCN
30 - 40 g/l KOH

Used at room temp. with steel anodes at 1 - 4 amps/dm2

Good luck  