TECHNET Archives

September 1999

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
Subject:
From:
Chris Evans <[log in to unmask]>
Date:
Tue, 28 Sep 1999 12:49:52 +0100
Content-Type:
multipart/alternative; boundary="openmail-part-0b0f3be3-00000002"
MIME-Version:
1.0
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, [log in to unmask]
Parts/Attachments:
BDY.RTF (509 bytes) , BDY.RTF (886 bytes)
Ken

Phosphorous content can vary from about 6% up to about 15% it depends on
the type of solution and how it is controlled. Some general points:

Some solutions are sold as high phosphorous ie < 10% P
The pH of the solution during processing effects the P content - low pH
high P
The hypophosphite content can effect it - high hypo - high P
For ease of solderability low phosphorous content is preferable.

Your processor should know about these effects otherwise how can he
control the solution!!