TECHNET Archives

September 2009

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Wenger, George M." <[log in to unmask]>
Date:
Tue, 22 Sep 2009 16:39:12 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Lee parker <[log in to unmask]>
Subject:
From:
Lee parker <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="iso-8859-1"
MIME-Version:
1.0
Parts/Attachments:
text/plain (294 lines)
George

Thank you for your interest. Actually I have seen these issues occur on nearly every finish except solder plated boards ( going back to the dark ages). The occurrence has diminished over the years, but it still happens. My guess is it may never be completely resolved as the first reaction is to point fingers at the other guy.

Best regards
Lee
J. L. Parker Ph. D.
JLP Consultants LLC
804 779 3389  
  ----- Original Message ----- 
  From: Wenger, George M.<mailto:[log in to unmask]> 
  To: TechNet E-Mail Forum<mailto:[log in to unmask]> ; Lee parker<mailto:[log in to unmask]> 
  Sent: Tuesday, September 22, 2009 4:31 PM
  Subject: RE: [TN] Imm Sn soldering issue.


  Lee,

  Okay now that I read you whole response I can see the issues you're
  talking about and they do have application with both surface finishes.
  It's just that when you said "you may have problems other than the
  immersion silver surface" I thought you misread what surface finish
  Peter asked his question about.

  Regards,
  George
  George M. Wenger
  Andrew Solutions
  Senior Principal FMA / Reliability Engineer
  40 Technology Drive, Warren, NJ 07059
  (908) 546-4531 [Office]  (732) 309-8964 [Cell]
  [log in to unmask]<mailto:[log in to unmask]>
   

  -----Original Message-----
  From: TechNet [mailto:[log in to unmask]] On Behalf Of Lee parker
  Sent: Tuesday, September 22, 2009 4:25 PM
  To: [log in to unmask]<mailto:[log in to unmask]>
  Subject: Re: [TN] Imm Sn soldering issue.

  George

  I am aware of that, but my suggests have potential application in either
  case.

  Best regards
  Lee
  J. L. Parker Ph. D.
  JLP Consultants LLC
  804 779 3389  
    ----- Original Message ----- 
    From: Wenger, George M.<mailto:[log in to unmask]<mailto:[log in to unmask]>> 
    To: TechNet E-Mail Forum<mailto:[log in to unmask]<mailto:[log in to unmask]>> ; Lee
  parker<mailto:[log in to unmask]<mailto:[log in to unmask]>> 
    Sent: Tuesday, September 22, 2009 3:21 PM
    Subject: RE: [TN] Imm Sn soldering issue.


    Lee,

    Peter is having problems with immersion TIN not immersion SILVER

    Regards,
    George
    George M. Wenger
    Andrew Solutions
    Senior Principal FMA / Reliability Engineer
    40 Technology Drive, Warren, NJ 07059
    (908) 546-4531 [Office]  (732) 309-8964 [Cell]
    [log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]:[log in to unmask]>>
     
    -----Original Message-----
    From: TechNet [mailto:[log in to unmask]] On Behalf Of Lee parker
    Sent: Tuesday, September 22, 2009 3:03 PM
    To: [log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]:[log in to unmask]>>
    Subject: Re: [TN] Imm Sn soldering issue.

    Peter you mentioned that the defects are normally on the second side.
  I
    was also wondering if the defects are usually associated with the same
    features. If so you may have problems other than the immersion silver
    surface. Issues I have uncovered are soldermask residues and soldering
    fixtures (if you are using fixtures) that prevent contact of the board
    and the solder. I suggest that the next time this occurs you process a
    bare board with no no soldermask or fixturing and see if you get the
    same result. Quite often I do not.

    Best regards
    Lee
    J. L. Parker Ph. D.
    JLP Consultants LLC
    804 779 3389
      ----- Original Message ----- 
      From: Peter Barton<mailto:[log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]:[log in to unmask]>>> 
      To:
  [log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]:T<mailto:[log in to unmask]:[log in to unmask]:[log in to unmask]:T>
  [log in to unmask]<mailto:[log in to unmask]>>> 
      Sent: Tuesday, September 22, 2009 12:33 PM
      Subject: [TN] Imm Sn soldering issue.


      Dear Technetters,

      Hopefully there is someone out there who can help me understand a
  very
    specific issue we have using PCB's plated with Imm Sn. namely,
    non-wetting of solder to some lands on the second side of population
    after reflow. We have an understanding of this surface finish with
    respect to the assembly processes. We are careful how we handle the
    unpopulated PCB's, the PCB's are shipped directly to the line and are
    only removed from the manufacturer's packaging at the point of use.
  They
    are not pre-baked and are subjected to 2 relatively benign reflow
    cycles.

      We only ever see the issue on the second side. It occurs on various
    component types. When it does occur the solder deposited at the
  printing
    stage is reflowed and is attached to the component termination,
    favouring this as more wettable than the PCB land. The problem does
  not
    always occur. The assembly is populated in 2 up panels and we have
    examples where one panel has soldered joints across the piece, whilst
    the other PCB in the same panel exhibits non wetting in some areas.

      The assembly has been profiled with a good distribution of
    thermocouples on a sample assembly to confirm a low delta T and the
    profile itself is right at the centre of the paste manufacturer's
    recommendations. We like to have a good process window.

      I am aware that the 2 possible reasons for this condition are (a)
    thermal degradation of the finish and (b) possible plating quality
    issues.

      We have dismissed excessive thermal input as these have only been
    subjected to 2 non-RoHS thermal cycles and the PCB's are fresh from
  the
    manufacturer. Peak temperatures are only around the 227 deg. C mark.
  The
    Sn thickness specification is 0.8 - 1.2 uM. The applied thickness has
    been measured using XRF as a process control and averages 1.0 uM. I am
    aware that XRF is only a guide as it cannot segregate out 'available'
    pure Sn from Sn/Cu intermetallics.

      We have had an independent lab analysis conducted and example lands
    where this condition is seen are shown to have very little or no
    remaining Sn at the surface, the majority being Sn/Cu intermetallics.
    Other unpopulated plated areas have also been subjected to SEM and EDX
    for comparison and exhibit what is described as 'islands' of Sn in a
  sea
    of Cu/Sn intermetallics.

      We have not had 'virgin' PCB's analysed yet for comparison as it is
    costly and we are not sure if we would pick the correct example to
  look
    at - it could be a good one.

      For the PCB experts out there out there I have a couple of
  questions:

      1. If the application of Sn is a displacement reaction with the
    underlying Cu is there any way that there can be less Sn on some
  surface
    areas than others?

      2. Are there other reasons that there could be variation in Sn
    deposits or could lead to the 'islands' of Sn as described by our lab
    that is seen after thermal processing?

      3. Are we missing anything else?

      Any questions please feel free to ask - this is causing me the
  biggest
    headache going.

      Peter Barton
      Senior Process Engineer
      ACW Technology Ltd
      Dinas Isaf West
      Tonypandy
      Mid Glamorgan
      CF40 1XX

      Tel: 01443 425275 (direct)
      Fax 02380 484882
   
  [log in to unmask]<mailto:[log in to unmask]<mailto:E-mail-pb21@wc<mailto:[log in to unmask]:[log in to unmask]:E-mail-pb21@wc>
  w.co.uk%3Cmailto:[log in to unmask]>>

      ---------------------------------------------------
      Technet Mail List provided as a service by IPC using LISTSERV 15.0
      To unsubscribe, send a message to
   
  [log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]:[log in to unmask]:[log in to unmask]>
  o:[log in to unmask]>> with following text in
      the BODY (NOT the subject field): SIGNOFF Technet
      To temporarily halt or (re-start) delivery of Technet send e-mail to
   
  [log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]:[log in to unmask]:[log in to unmask]>
  o:[log in to unmask]>>: SET Technet NOMAIL or (MAIL)
      To receive ONE mailing per day of all the posts: send e-mail to
   
  [log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]:[log in to unmask]:[log in to unmask]>
  o:[log in to unmask]>>: SET Technet Digest
      Search the archives of previous posts at:
   
  http://listserv.ipc.org/archives<http://listserv.ipc.org/archives<http:/<http://listserv.ipc.org/archives%3Chttp://listserv.ipc.org/archives%3Chttp:/>
  /listserv.ipc.org/archives%3Chttp://listserv.ipc.org/archives>>
      Please visit IPC web site
   
  http://www.ipc.org/contentpage.asp?Pageid=4.3.16<http://www.ipc.org/cont<http://www.ipc.org/contentpage.asp?Pageid=4.3.16<http://www.ipc.org/cont>
  <http://www.ipc.org/contentpage.asp?Pageid=4.3.16<http://www.ipc.org/con<http://www.ipc.org/contentpage.asp?Pageid=4.3.16<http://www.ipc.org/con>
  t>
    entpage.asp?Pageid=4.3.16> for additional information, or contact
  Keach
    Sasamori at
  [log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]:sasa<mailto:[log in to unmask]:[log in to unmask]:[log in to unmask]:sasa>
  [log in to unmask]<mailto:[log in to unmask]>>> or 847-615-7100
    ext.2815
      -----------------------------------------------------

    ---------------------------------------------------
    Technet Mail List provided as a service by IPC using LISTSERV 15.0
    To unsubscribe, send a message to
  [log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]:[log in to unmask]>> with following text
    in
    the BODY (NOT the subject field): SIGNOFF Technet
    To temporarily halt or (re-start) delivery of Technet send e-mail to
    [log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]:[log in to unmask]>>: SET Technet NOMAIL or
  (MAIL)
    To receive ONE mailing per day of all the posts: send e-mail to
    [log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]:[log in to unmask]>>: SET Technet Digest
    Search the archives of previous posts at:
    http://listserv.ipc.org/archives<http://listserv.ipc.org/archives<http://listserv.ipc.org/archives%3Chttp://listserv.ipc.org/archives>>
    Please visit IPC web site
   
  http://www.ipc.org/contentpage.asp?Pageid=4.3.16<http://www.ipc.org/cont<http://www.ipc.org/contentpage.asp?Pageid=4.3.16<http://www.ipc.org/cont>
  entpage.asp?Pageid=4.3.16> for additional
    information, or contact Keach Sasamori at
  [log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]:[log in to unmask]>> or 847-615-7100
    ext.2815
    -----------------------------------------------------

   
  ------------------------------------------------------------------------
  ------------------------
    This message is for the designated recipient only and may
    contain privileged, proprietary, or otherwise private information.  
    If you have received it in error, please notify the sender
    immediately and delete the original.  Any unauthorized use of
    this email is prohibited.
   
  ------------------------------------------------------------------------
  ------------------------
    [mf2]


  ---------------------------------------------------
  Technet Mail List provided as a service by IPC using LISTSERV 15.0
  To unsubscribe, send a message to [log in to unmask]<mailto:[log in to unmask]> with following text
  in
  the BODY (NOT the subject field): SIGNOFF Technet
  To temporarily halt or (re-start) delivery of Technet send e-mail to
  [log in to unmask]<mailto:[log in to unmask]>: SET Technet NOMAIL or (MAIL)
  To receive ONE mailing per day of all the posts: send e-mail to
  [log in to unmask]<mailto:[log in to unmask]>: SET Technet Digest
  Search the archives of previous posts at:
  http://listserv.ipc.org/archives<http://listserv.ipc.org/archives>
  Please visit IPC web site
  http://www.ipc.org/contentpage.asp?Pageid=4.3.16<http://www.ipc.org/contentpage.asp?Pageid=4.3.16> for additional
  information, or contact Keach Sasamori at [log in to unmask]<mailto:[log in to unmask]> or 847-615-7100
  ext.2815
  -----------------------------------------------------

  ------------------------------------------------------------------------------------------------
  This message is for the designated recipient only and may
  contain privileged, proprietary, or otherwise private information.  
  If you have received it in error, please notify the sender
  immediately and delete the original.  Any unauthorized use of
  this email is prohibited.
  ------------------------------------------------------------------------------------------------
  [mf2]


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2