TECHNET Archives

September 2009

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Lee parker <[log in to unmask]>
Date:
Tue, 22 Sep 2009 16:31:41 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Wenger, George M." <[log in to unmask]>
Subject:
From:
"Wenger, George M." <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (279 lines)
Okay now that I read you whole response I can see the issue
Lee,



Okay now that I read you whole response I can see the issues you're

talking about and they do have application with both surface finishes.

It's just that when you said "you may have problems other than the

immersion silver surface" I thought you misread what surface finish

Peter asked his question about.



Regards,

George

George M. Wenger

Andrew Solutions

Senior Principal FMA / Reliability Engineer

40 Technology Drive, Warren, NJ 07059

(908) 546-4531 [Office]  (732) 309-8964 [Cell]

[log in to unmask]

 



-----Original Message-----

From: TechNet [mailto:[log in to unmask]] On Behalf Of Lee parker

Sent: Tuesday, September 22, 2009 4:25 PM

To: [log in to unmask]

Subject: Re: [TN] Imm Sn soldering issue.



George



I am aware of that, but my suggests have potential application in either

case.



Best regards

Lee

J. L. Parker Ph. D.

JLP Consultants LLC

804 779 3389  

  ----- Original Message ----- 

  From: Wenger, George M.<mailto:[log in to unmask]> 

  To: TechNet E-Mail Forum<mailto:[log in to unmask]> ; Lee

parker<mailto:[log in to unmask]> 

  Sent: Tuesday, September 22, 2009 3:21 PM

  Subject: RE: [TN] Imm Sn soldering issue.





  Lee,



  Peter is having problems with immersion TIN not immersion SILVER



  Regards,

  George

  George M. Wenger

  Andrew Solutions

  Senior Principal FMA / Reliability Engineer

  40 Technology Drive, Warren, NJ 07059

  (908) 546-4531 [Office]  (732) 309-8964 [Cell]

  [log in to unmask]<mailto:[log in to unmask]>

   

  -----Original Message-----

  From: TechNet [mailto:[log in to unmask]] On Behalf Of Lee parker

  Sent: Tuesday, September 22, 2009 3:03 PM

  To: [log in to unmask]<mailto:[log in to unmask]>

  Subject: Re: [TN] Imm Sn soldering issue.



  Peter you mentioned that the defects are normally on the second side.

I

  was also wondering if the defects are usually associated with the same

  features. If so you may have problems other than the immersion silver

  surface. Issues I have uncovered are soldermask residues and soldering

  fixtures (if you are using fixtures) that prevent contact of the board

  and the solder. I suggest that the next time this occurs you process a

  bare board with no no soldermask or fixturing and see if you get the

  same result. Quite often I do not.



  Best regards

  Lee

  J. L. Parker Ph. D.

  JLP Consultants LLC

  804 779 3389

    ----- Original Message ----- 

    From: Peter Barton<mailto:[log in to unmask]<mailto:[log in to unmask]>> 

    To:

[log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]:T

[log in to unmask]>> 

    Sent: Tuesday, September 22, 2009 12:33 PM

    Subject: [TN] Imm Sn soldering issue.





    Dear Technetters,



    Hopefully there is someone out there who can help me understand a

very

  specific issue we have using PCB's plated with Imm Sn. namely,

  non-wetting of solder to some lands on the second side of population

  after reflow. We have an understanding of this surface finish with

  respect to the assembly processes. We are careful how we handle the

  unpopulated PCB's, the PCB's are shipped directly to the line and are

  only removed from the manufacturer's packaging at the point of use.

They

  are not pre-baked and are subjected to 2 relatively benign reflow

  cycles.



    We only ever see the issue on the second side. It occurs on various

  component types. When it does occur the solder deposited at the

printing

  stage is reflowed and is attached to the component termination,

  favouring this as more wettable than the PCB land. The problem does

not

  always occur. The assembly is populated in 2 up panels and we have

  examples where one panel has soldered joints across the piece, whilst

  the other PCB in the same panel exhibits non wetting in some areas.



    The assembly has been profiled with a good distribution of

  thermocouples on a sample assembly to confirm a low delta T and the

  profile itself is right at the centre of the paste manufacturer's

  recommendations. We like to have a good process window.



    I am aware that the 2 possible reasons for this condition are (a)

  thermal degradation of the finish and (b) possible plating quality

  issues.



    We have dismissed excessive thermal input as these have only been

  subjected to 2 non-RoHS thermal cycles and the PCB's are fresh from

the

  manufacturer. Peak temperatures are only around the 227 deg. C mark.

The

  Sn thickness specification is 0.8 - 1.2 uM. The applied thickness has

  been measured using XRF as a process control and averages 1.0 uM. I am

  aware that XRF is only a guide as it cannot segregate out 'available'

  pure Sn from Sn/Cu intermetallics.



    We have had an independent lab analysis conducted and example lands

  where this condition is seen are shown to have very little or no

  remaining Sn at the surface, the majority being Sn/Cu intermetallics.

  Other unpopulated plated areas have also been subjected to SEM and EDX

  for comparison and exhibit what is described as 'islands' of Sn in a

sea

  of Cu/Sn intermetallics.



    We have not had 'virgin' PCB's analysed yet for comparison as it is

  costly and we are not sure if we would pick the correct example to

look

  at - it could be a good one.



    For the PCB experts out there out there I have a couple of

questions:



    1. If the application of Sn is a displacement reaction with the

  underlying Cu is there any way that there can be less Sn on some

surface

  areas than others?



    2. Are there other reasons that there could be variation in Sn

  deposits or could lead to the 'islands' of Sn as described by our lab

  that is seen after thermal processing?



    3. Are we missing anything else?



    Any questions please feel free to ask - this is causing me the

biggest

  headache going.



    Peter Barton

    Senior Process Engineer

    ACW Technology Ltd

    Dinas Isaf West

    Tonypandy

    Mid Glamorgan

    CF40 1XX



    Tel: 01443 425275 (direct)

    Fax 02380 484882

 

[log in to unmask]<mailto:[log in to unmask]<mailto:E-mail-pb21@wc

w.co.uk%3Cmailto:[log in to unmask]>>



    ---------------------------------------------------

    Technet Mail List provided as a service by IPC using LISTSERV 15.0

    To unsubscribe, send a message to

 

[log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]

o:[log in to unmask]>> with following text in

    the BODY (NOT the subject field): SIGNOFF Technet

    To temporarily halt or (re-start) delivery of Technet send e-mail to

 

[log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]

o:[log in to unmask]>>: SET Technet NOMAIL or (MAIL)

    To receive ONE mailing per day of all the posts: send e-mail to

 

[log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]

o:[log in to unmask]>>: SET Technet Digest

    Search the archives of previous posts at:

 

http://listserv.ipc.org/archives<http://listserv.ipc.org/archives<http:/

/listserv.ipc.org/archives%3Chttp://listserv.ipc.org/archives>>

    Please visit IPC web site

 

http://www.ipc.org/contentpage.asp?Pageid=4.3.16<http://www.ipc.org/cont

<http://www.ipc.org/contentpage.asp?Pageid=4.3.16<http://www.ipc.org/con

t>

  entpage.asp?Pageid=4.3.16> for additional information, or contact

Keach

  Sasamori at

[log in to unmask]<mailto:[log in to unmask]<mailto:[log in to unmask]:sasa

[log in to unmask]>> or 847-615-7100

  ext.2815

    -----------------------------------------------------



  ---------------------------------------------------

  Technet Mail List provided as a service by IPC using LISTSERV 15.0

  To unsubscribe, send a message to

[log in to unmask]<mailto:[log in to unmask]> with following text

  in

  the BODY (NOT the subject field): SIGNOFF Technet

  To temporarily halt or (re-start) delivery of Technet send e-mail to

  [log in to unmask]<mailto:[log in to unmask]>: SET Technet NOMAIL or

(MAIL)

  To receive ONE mailing per day of all the posts: send e-mail to

  [log in to unmask]<mailto:[log in to unmask]>: SET Technet Digest

  Search the archives of previous posts at:

  http://listserv.ipc.org/archives<http://listserv.ipc.org/archives>

  Please visit IPC web site

 

http://www.ipc.org/contentpage.asp?Pageid=4.3.16<http://www.ipc.org/cont

entpage.asp?Pageid=4.3.16> for additional

  information, or contact Keach Sasamori at

[log in to unmask]<mailto:[log in to unmask]> or 847-615-7100

  ext.2815

  -----------------------------------------------------



 

------------------------------------------------------------------------

------------------------

  This message is for the designated recipient only and may

  contain privileged, proprietary, or otherwise private information.  

  If you have received it in error, please notify the sender

  immediately and delete the original.  Any unauthorized use of

  this email is prohibited.

 

------------------------------------------------------------------------

------------------------

  [mf2]





---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text

in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to

[log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to

[log in to unmask]: SET Technet Digest

Search the archives of previous posts at:

http://listserv.ipc.org/archives

Please visit IPC web site

http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional

information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100

ext.2815

-----------------------------------------------------



------------------------------------------------------------------------------------------------

This message is for the designated recipient only and may

contain privileged, proprietary, or otherwise private information.  

If you have received it in error, please notify the sender

immediately and delete the original.  Any unauthorized use of

this email is prohibited.

------------------------------------------------------------------------------------------------

[mf2]



---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2