Ken,
Reflow pad width no wider than nominal chip width, pad length 1 mm, pad
separation 1 mm or pad ctr to ctr dimension 2 mm or nominal chip length.
Stencil thickness should be 4-5 mils and a home plate stencil should be
used to minimize any solder balls during reflow soldering.
Wave solder pad width should be 1/2 to 2/3 nominal chip width and extend
beyond the chip end 1 1/2 time chip thickness.
John
>John,
>
>Not being a board designer, what is the recommended pad size and geometry
>for a ceramic 0805?
>
>Thanks,
>
>KennyB
>
>-----Original Message-----
>From: John Maxwell [mailto:[log in to unmask]]
>Sent: Monday, April 28, 2008 3:04 PM
>To: TechNet E-Mail Forum; Ken Bloomquist
>Subject: Re: [TN] Cracking Ceramic Cap
>
>Ken,
>Boy this take me back to my capacitor cracking days. It will be nice to
>see what the failures look like but from what has been described is
>consistent with assembly flexure cracking. When I wrote my first paper
>on MLCC crack signatures the great majority of cracks were due to
>assembly handling followed closely be excessive solder joint size.
>Things have not changed in the intervening 20+ years. Big wide solder
>joints and a connector right next door, the perfect recipe for cracks.
>
>John Maxwell
>
>
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
>Search the archives of previous posts at: http://listserv.ipc.org/archives
>Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
>-----------------------------------------------------
>
>
>
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|