TECHNET Archives

October 2008

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
"Igoshev, Vladimir" <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Igoshev, Vladimir
Date:
Fri, 10 Oct 2008 09:39:57 -0400
Content-Type:
text/plain
Parts/Attachments:
text/plain (1 lines)
Werner,



I believe I saw a similar failure on a board from the same board shop and it WAS NOT BP. :-)



Regards,



Vladimir



----- Original Message -----

From: TechNet <[log in to unmask]>

To: [log in to unmask] <[log in to unmask]>

Sent: Fri Oct 10 09:34:54 2008

Subject: Re: [TN] PCB pad non-wetting issues





 

-----------------------------------------------------

Hi Paymon,

The root cause is ENIG 'Black Pad.'

In order to protect the electroless Ni from the immersion Au plating bath, P is codeposited. 

As more and more Ni is dissolved during numerous soldering processes more P is left behind 

weakening the interfacial structure--the more P, te weaker the interface.



Werner







 





 



-----Original Message-----

From: Paymon Sani <[log in to unmask]>

To: [log in to unmask]

Sent: Thu, 9 Oct 2008 9:57 am

Subject: [TN] PCB pad non-wetting issues





















Hello All,



 



We are experiencing a pad non-wetting issue for the though-hole

component pads ONLY! The PCB goes through few heat cycles with top and

bottom side assembly during at SMT process and then through-hole

assembly at wave process. The problem is found at Wave process. The Pb

solder does not wet to the through-hole component pads on the solder

side only! An SEM/EDS evaluation revealed high concentration of P in the

Nickel and Nickel/Tin intermetalic layer of 11% to 21%. I would like to

ask anyone if they have experienced a similar defect in the past. What

is the Root Cause?



 



Thank you in advance,



Paymon





---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to 

[log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to 

[log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for 

additional information, or contact Keach Sasamori at [log in to unmask] or 

847-615-7100 ext.2815









 





---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815

-----------------------------------------------------




ATOM RSS1 RSS2