TECHNET Archives

March 1997

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Received:
by ipc.org (Smail3.1.28.1 #2) id m0w4Lyb-000BBhC; Tue, 11 Mar 97 01:28 CST
From [log in to unmask] Tue Mar 11 08:
42:36 1997
Old-Return-Path:
Date:
Mon, 10 Mar 1997 15:28:43 -0500 (EST)
MIME-version:
1.0
Precedence:
list
Resent-From:
Cc:
X-Status:
Status:
O
X-Mailing-List:
<[log in to unmask]> archive/latest/11008
TO:
Return-Path:
<TechNet-request>
Content-type:
TEXT/PLAIN; CHARSET=US-ASCII
Subject:
From:
Allen Hertz <[log in to unmask]>
X-Loop:
Resent-Message-ID:
<"EbRMv.0.7p8.0cG9p"@ipc>
Message-id:
Resent-Sender:
TechNet-request [log in to unmask]
Parts/Attachments:
TEXT/PLAIN (53 lines)
In my past life, we used selectively plated gold with Entek CU106-A successfully 
for pressure contacts and switch contacts (to carbon ink actuators) without 
issue. The gold was bussed in prior to the OSP application.

Some assembly houses are concerened regaring reflowing on immersion gold, as on 
occasion, the solderability is not acceptable. N2 helps somewhat. The process 
controls are vendor dependant.

Regards,
Allen

_______________________________________________________________________________

Subject: Selective PCB plating

From:    [log in to unmask] at ftl03

Date:    3/10/97  2:28 PM



Does anyone know if you can selectively plate with OSPs and Immersion 
gold on the same PCB?  I would like to do immersion gold on my keypad 
contacts but use something Like Entek on the rest of the PCB.  Is this 
possible?  

My PCB assembly vendor doesn't like reflowing immersion gold PCBs.  He 
claims the solder doesn't flow very well.  Is it just him or the rest of 
the industry?

***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]>   *
* with <subject: subscribe/unsubscribe> and no text in the body.          *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact   *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask]      *
***************************************************************************


***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]>   *
* with <subject: subscribe/unsubscribe> and no text in the body.          *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact   *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask]      *
***************************************************************************



ATOM RSS1 RSS2