Steve,
I'm a big fan of XRF for material identification and plating thickness
measurements. We use our XRF to measure Sn or Sn and Cu or Sn and Ni
over steel, IAg or IAu and ENi or SnPb solder over copper. The problem
with XRF is you need to have calibration samples and you have thickness
limitations. For SnPb solder you're limited to less than 1500-2000 micro
inches (1.5 to 2.0 mils) and in my mine the accuracy above 1 mil is
questionable. Because we primarily use the XRF for immersion silver
(IAg), immersion gold (IAu), tin (Sn) and solder (SnPb) plating
measurements we have many standards for calibration. The vendors of XRF
equipment will tell you their equipment is "good" to +/-5%. However
they usually don't give you enough information to know +/-5% of what.
We've found that we can be within +/-5% of the values we calibrate with.
For example, if we calibrate our XRF for gold over nickel and our
standards are 50 micro inches of gold over 400 micro inches of nickel
our gold measurement accuracy is at best are +/- 2.5 micro inches and
nickel is +/-20 micro inches. That accuracy isn't bad considering that
that's about the accuracy of cross sectioning unless you take special
care in sample preparation and then use an SEM to measure.
Sorry for the long winded answer. The short answer would have been no
we don't use our XRF to measure copper trace thickness. We routinely
use an optical microscope with X-Y-Z measurement capability at 400x
magnification to measure the copper trace thickness.
Regards,
George
George M. Wenger Andrew Corporation
40 Technology Drive, Warren, NJ 07059
(908) 546-4531 [log in to unmask]
-----Original Message-----
From: Steve Gregory [mailto:[log in to unmask]]
Sent: Friday, June 06, 2003 4:13 PM
To: [log in to unmask]
Subject: Re: [TN] Technical Question about Materials Labs
Hi George!
Me not being much of a lab person, I got a response to my trace
thickness post recently, that XRF is not a good tool to measure copper
trace thickness. Is this true?
Thanks!
-Steve Gregory-
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
------------------------------------------------------------------------------------------------
This message is for the designated recipient only and may
contain privileged, proprietary, or otherwise private information.
If you have received it in error, please notify the sender
immediately and delete the original. Any unauthorized use of
this email is prohibited.
------------------------------------------------------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
[mf2]
|
|
|