TECHNET Archives

November 2006

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
"Bloomquist, Ken" <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Bloomquist, Ken
Date:
Thu, 2 Nov 2006 13:52:08 -0800
Content-Type:
text/plain
Parts/Attachments:
text/plain (36 lines)
That's just great; we get to redesign all the circuit boards in the
world in order to be successful at soldering SMT assemblies! No cost
involved there that I can see!

That should be some more cannon fodder for John and "Push Back"!

KennyB

-----Original Message-----
From: Werner Engelmaier [mailto:[log in to unmask]] 
Sent: Thursday, November 02, 2006 1:33 PM
To: [log in to unmask]
Subject: Re: [TN] Bizzare Phenomena...

Hi Steve,

Tombstoning is worse for LF-solders than for SnPb.
The surest way of eliminating tombstoning entirely is by eliminating the
fillets--make the pads the same size as the metallization on the CC
underside [or
just slightly larger]. No more tombstoning, no more CC cracking and more
reliable solder joints as well because you wind up with more solder
joint height.

Werner

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2