Received: |
by ipc.org (Smail3.1.28.1 #2)
id m0wUBnD-000BjBC; Wed, 21 May 97 08:51 CDT |
Content-Type: |
text/plain; charset=US-ASCII |
Old-Return-Path: |
|
Date: |
Wed, 21 May 97 09:13:08 -0600 |
Precedence: |
list |
Resent-From: |
|
Resent-Sender: |
|
From [log in to unmask] Wed May 21 10: |
51:33 1997 |
Status: |
O |
>From bergdi Wed May 21 08: |
51:38 1997 |
TO: |
|
Return-Path: |
<TechNet-request> |
X-Status: |
|
X-Loop: |
|
X-Mailing-List: |
|
Resent-Message-ID: |
<"Eju-r3.0.nfB.2tlWp"@ipc> |
Subject: |
|
From: |
|
Content-Transfer-Encoding: |
7bit |
MIME-Version: |
1.0 |
X-Mailer: |
ccMail Link to SMTP R6.00.02 |
Message-Id: |
|
Parts/Attachments: |
|
|
Is the rubber real rubber or plastic? Many plastics are degrade
slightly and release sulfuric acid. (Paper does this also, look at any
old newspaper. The yellow color is from the acid.)
There are also might be some unbound sulfur in the rubber, left from
the vulcanization process.
______________________________ Reply Separator _________________________________
Subject: Copper Sulphide corrosion
Author: <[log in to unmask]> at internet
Date: 5/21/97 2:07 PM
Hi
We have seen failures on a bought-in assembly due to growth of copper
sulphide on the copper traces of a flexible PCB. The failure occurs at the
base of SnPb solder joints, where the copper traces are not covered by
photoresist. The whole area of exposed copper and solder joints is covered
by a silicone based potting material.
Unfortunately our supplier is not being very helpful, so I am looking for
clues as to what is happening and how to stop it myself.
The source of sulphur is not known, but there are various rubber components
within the immediate area.
Does anyone have any experience of this type of corrosion system? If so, I
would appreciate a discussion about the factors involved - in particular,
the role of the potting compound and whether an alternative passivating
material would do a better job.
Thank you
John Loveluck
Group Quality Manager
Tadpole Technology plc
Cambridge Science Park
Cambridge CB4 4RB
Tel: (+44)1223.428200
Fax: (+44)1223.428201
email: [log in to unmask]
***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]> *
* with <subject: subscribe/unsubscribe> and no text in the body. *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] *
***************************************************************************
***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]> *
* with <subject: subscribe/unsubscribe> and no text in the body. *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] *
***************************************************************************
|
|
|