Bill,
If you have not already, look at the cooling rate on your reflow oven. I
solved a similar similar warpage problem by reducing the solder cooling rate
to 1 deg C/second. I had to modify the blowers in the cool down section to
achieve that rate. I found my oven was designed to blast the top of the BGA
with cold air while the solder was still liquidus. It provided for high
speed production, but was warping some of the BGA's.
Jim Kittel
-----Original Message-----
From: Bill Raymond [mailto:[log in to unmask]]
Sent: Thursday, September 06, 2001 6:16 AM
To: [log in to unmask]
Subject: Re: [TN] BGA Warp
Werner, thanks for your comments. We are stuck with a single source for
this BGA... no one else makes it. Looks like my best bet is to try to talk
to the "right" person at the BGA manufacturer.
Bill...
At 03:56 AM 09/06/2001 -0400, you wrote:
>Hi Bill,
>BGA warpage is the consequence of an asymmetric [=bad] design. My
>recommendation, get somebody else's BGA.
>Werner Engelmaier
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|