TECHNET Archives

November 2006

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Steve Gregory <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Steve Gregory <[log in to unmask]>
Date:
Thu, 2 Nov 2006 06:46:16 -0600
Content-Type:
text/plain
Parts/Attachments:
text/plain (122 lines)
Mornin' Les!

Gracious no! None of our military customers are lead-free...

-Steve- 

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of - Bogert
Sent: Wednesday, November 01, 2006 5:35 PM
To: [log in to unmask]
Subject: Re: [TN] Bizzare Phenomena...

November 1, 2006

I can offer no help Steve, but can you tell me if your lead-free
customers are military equipment?
  ----- Original Message -----
  From: Steve Gregory<mailto:[log in to unmask]>
  To: [log in to unmask]<mailto:[log in to unmask]>
  Sent: Tuesday, October 31, 2006 9:57 AM
  Subject: [TN] Bizzare Phenomena...


  Mornin' All!
   
  This morning I have seen something that I have never, ever have seen
  before. It's been a little slow the past week, so we decided to do our
  maintenance on our reflow ovens. After we opened the oven up, we found
  many, many solderballs laying on the bottom of the oven right around
  zone 7 - 8, right at the beginning of the spike zone. Check-out:
   
 
http://stevezeva.homestead.com/files/Oven_Solderballs.jpg<http://steveze
va.homestead.com/files/Oven_Solderballs.jpg>
   
 
http://stevezeva.homestead.com/files/Oven_Solderballs_2.jpg<http://steve
zeva.homestead.com/files/Oven_Solderballs_2.jpg>
   
 
http://stevezeva.homestead.com/files/Oven_Solderballs_3.jpg<http://steve
zeva.homestead.com/files/Oven_Solderballs_3.jpg>
   
 
http://stevezeva.homestead.com/files/Oven_Solderballs_4.jpg<http://steve
zeva.homestead.com/files/Oven_Solderballs_4.jpg>
   
  We've been having tombstoning problems when we've run the two
lead-free
  jobs that we have here. I've been working with the paste vendor
sending
  my profiles and plots, but I haven't been able to solve the problem.
The
  solderballs in the oven are lead-free solderballs.
   
  We are using a Heller 1809, and my profile set-points are:
   
  120    140    160    180    190    200    230    240    250
  120    140    160    180    190    200    230    240    250
   
  Belt speed 26 in per min
   
  The paste is a SAC 305 with a water washable no-clean flux. I think my
  profile is pretty reasonable, and the last board we ran is pretty
  standard, .062" thick, with no bizzare copper planes. The board finish
  with both jobs has been ENIG. The last job I ran we were tombstoning
  0805's, the one before that we were tombstoning 0402's. With both jobs
  we've had major tombstoning problems. I've slowed the beltspeed down,
  sped it up, ramped up slower, ramped up faster, changed this, changed
  that, but still haven't resolved my tombstoning.
   
  Of course, I'm the only one that's having this problem according to my
  paste vendor... 
   
  I wouldn't have imagined that I would see the solderballs in the oven
  like we have...
   
  Have any of you ever seen something like this before?
   
  -Steve Gregory-

  ---------------------------------------------------
  Technet Mail List provided as a service by IPC using LISTSERV 1.8e
  To unsubscribe, send a message to
[log in to unmask]<mailto:[log in to unmask]> with following text in
  the BODY (NOT the subject field): SIGNOFF Technet
  To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]<mailto:[log in to unmask]>: SET Technet NOMAIL or (MAIL)
  To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]<mailto:[log in to unmask]>: SET Technet Digest
  Search the archives of previous posts at:
http://listserv.ipc.org/archives<http://listserv.ipc.org/archives>
  Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16<http://www.ipc.org/cont
entpage.asp?Pageid=4.3.16> for additional information, or contact Keach
Sasamori at [log in to unmask]<mailto:[log in to unmask]> or 847-615-7100
ext.2815
  -----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2