TECHNET Archives

August 2012

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Joyce Koo <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Joyce Koo <[log in to unmask]>
Date:
Wed, 8 Aug 2012 12:20:28 +0000
Content-Type:
text/plain
Parts/Attachments:
text/plain (30 lines)
Thanks.  Tom and Brian.  

Joyce Koo
Materials Researcher - Materials Interconnect Lab
Research In Motion Limited
Office: (519) 888-7465 79945
Mobile: (226) 220-4760


-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Brian Chandler
Sent: Wednesday, August 08, 2012 8:14 AM
To: [log in to unmask]
Subject: Re: [TN] pin in paste

We use Pin In Paste on many automotive products. Some things that come to mind are:
- Controlling the pin to hole ratio. Keep it between 0.3 - 0.5
- Limiting the lead protrusion to 1.5mm maximum
- No 'kinked' leads in the PTH, straight leads only

Good luck!

---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2