Tom
Get rid of your Ni-barrier and you problems will go away....
If you insist on using a Ni barrier, watch your O and C levels for O2 diffusion and Cx for contaminates between your Ni and Au layers...
Paul
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Gervascio, Thomas
Sent: Wednesday, March 19, 2008 12:08 PM
To: [log in to unmask]
Subject: [TN] Case of the popping BGAs
Want to ask the advice of the Learned Forum members. Had an experience
where BGAs were falling off CCAs after shipment. Both the solder and the
solder balls are Sn63/Pb 37 solder alloy. Had the parts and boards
tested by a third party lab. Their results are
"The following report is in regards to the failure analysis of the two
largest BGA components on failed
assembly . The following lists the analyses performed in the attempt to
determine the root cause of the separation of the BGA components from
the assembly:
- SEM/EDS surface analysis of the failed PCB sites
-SEM/EDS surface analysis of the corresponding failed BGA component
sites
-Micro-sectional/SEM evaluation of the failed PCB sites
-Micro-sectional/SEM evaluation of the corresponding failed BGA
component sites
All evaluations were performed with a Camscan MV2300 thermionic emission
scanning electron microscope (SEM), fitted with an Oxford EDS system
(elementalanalysis). The images obtained during the analysis can be
found in the following pages.
Note: All micro-section samples were exposed to a chemical tin and
copper etch, to better visualize
the intermetallic layer (IMC).
Results:
SEM/EDS surface analysis
The following tables show the EDS results (in weight%) of five randomly
chosen sites on the failed PCB and failed component site respectively.
All analysis was obtained at 10kV acceleration potential
(ND = Not Detected):
PCB site/small BGA
Pad Ni Sn P C O
1 74.5 3.9 6.6 13.8 1.2
2 75.7 3.7 6.9 12.7 1.0
3 78.8 4.0 7.3 9.9 ND
4 77.7 4.1 6.8 11.4 ND
5 81.1 3.6 7.9 7.5 ND
PCB site/large BGA
Pad Ni Sn P C O
1 80 3 .2 4 .7 11.3 0.9
2 81.1 2.4 5.3 11.3 ND
3 72 4.3 6.7 15.9 1.1
4 77.5 4.9 7.4 10.3 ND
5 78 5.5 7.5 8.9 ND
Component site/small BGA
Pad Ni Sn Pb C O P
1 42.9 24. 8.1 23.6 7.1 0.6
2 25.1 23 5.1 32.7 13.7 0.3
3 42.8 26 2.4 22.4 5.9 0.5
4 49.8 28.3 1.5 16.5 3.3 0.6
5 35.5 20.7 1.4 31.1 10.8 0.5
Component site/large BGA
Pad Ni Sn Pb C O P
1 42.3 27.3 1.7 23.2 5.0 0.4
2 37.9 23.3 1.3 28.6 8.3 0.6
3 40.7 26.4 1.8 25.2 5.4 0.5
4 47.4 29.2 2.4 16 4.3 0.6
5 38.7 25.3 2.8 24.7 8.4 0.2
Small BGA:
PCB site; very thin areas of IMC were detected, but too thin to measure.
Nickel thickness was measured to be approximately 133 micro-inches. No
signs of nickel corrosion were detected.
Component site; an average of 2.09um of IMC layer thickness was measured
on a total of three BGA solder balls evaluated. All solder balls showed
proper ball collapse and IMC formation, indicating a sufficiently hot
assembly reflow profile.
Large BGA:
PCB site; very thin areas of IMC were detected, but too thin to measure.
No signs of nickel corrosion were detected.
Component site; an average of 1.52um of IMC layer thickness was measured
on a total of three BGA solder balls evaluated. All solder balls showed
proper ball collapse and IMC formation, indicating a sufficiently hot
assembly reflow profile.
,
What levels of Phosphorus would be expected in a nickel plating that
exhibits Black Pad? Any other ideas relating to the failure mechanism
and methods to validate them?
Thanks
Tom
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
==============================================================================
This email and any attachments thereto may contain private, confidential, and
privileged material for the sole use of the intended recipient. Any review, copying,
or distribution of this email (or any attachments thereto) by others is strictly prohibited.
If you are not the intended recipient, please contact [log in to unmask]
immediately and permanently delete the original and any copies of this email and
any attachments thereto.
==============================================================================
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|