TECHNET Archives

November 2006

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Wed, 22 Nov 2006 12:19:06 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Dehoyos, Ramon" <[log in to unmask]>
Subject:
From:
"Dehoyos, Ramon" <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="us-ascii"
MIME-Version:
1.0
Parts/Attachments:
text/plain (49 lines)
        Hi Werner:
                  You are right, thanks for correcting me. At SAC
profiles the SAC ball and the SnPb should melt together. On the other
hand, there are plenty of papers written about the negatives of mixing
SAC and SnPb. Don't you agree that it is not a good combination? One
more thing, Flux for SnPb is formulated to withstand SnPb profiles and
not SAC profiles. 
        Regards,
        Ramon 

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier
Sent: Monday, November 20, 2006 3:00 PM
To: [log in to unmask]
Subject: Re: [TN] FW: [TN] BGA anomaly

Hi Ramon,
Something sure got mixed-up somewhere. You say "BGA ball-solder
interface"; there is no such thing in a properly soldered SJ, and there
certainly are no IMCs there.. 
Some people have referred to this 'interface' on solder joints that did
not get hot enough for the solder volume to join up-and there may be
some flux remains there, but that is not the root cause.

Werner

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2