I'd have to assume that the caps that are cracking are ceramic chip caps,
and likely 0805 or larger.
I'd also bet you that the caps are near the edge of a board (vgroove?
perforations? shear?) or at another boundary at depanelization.
or:
They're near a connector that requires a deal of force to insert or
withdraw
or:
They're being flexed in test/burn in, etc.
or:
They're near a location where something's eyeletted or riveted.
or....
You've got some thermal shock conditions at wave/reflow
or
(you get the picture)
After many years years of working ceramic caps failures (among many others
:-) ), the the VAST majority (>95%) failed due to strain/stress being
induced in some step of the board mfg process.... mostly depanelization
and/or test.
Rgds
John
Square D Component Engineering
---------------------------------------------------------------------------------
DesignerCouncil Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF DesignerCouncil.
To set a vacation stop for delivery of DesignerCouncil send: SET DesignerCouncil NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|