Joe: This galvanic reaction is known as bimetallic corrosion. It takes place
when dissimilar metals are in contact with each other in the presence of an
electrolyte. In your case the copper is acting as an anode and being
deplated away in the microetch.
Here are some things to consider that will help.
1. Minimize the difference in surface area between the Au and Cu features.
Think of it as anode to cathode ratio. Make the anode(Cu) bigger than the
cathode(Au). Don't run small Cu traces into large Au pads if possible.
2. Minimize the time/concentration/temp of the microetch. In your earlier
posting you stated you where trying to remove 60u". That is a lot of Cu.
What is it you are trying to prep the surface for?
At one time in our OSP line we ran our peroxysulfuric micoetch at excessive
immersion times based on vendor recommendations. We had similar etchout
experiences, as you are seeing, on Cu/Au boards. We now run this process
using 30 sec. Vs the original 4 mins. in the micoetch. This removes about
5u" of Cu based on the chemistry concentration and temp for our microetch
bath. This has eliminated the severe etchout problem and has not affected
board finish or solderabiluty quality. You may want to consider a similar
approach.
3. Whenever possible cover exposed Cu and Cu/Au interface areas with
soldermask. This will help prevent localized etchout.
Regards
Michael Barmuta
Staff Engineer
Fluke Corp.
Everett Wa.
425-356-6076
-----Original Message-----
From: Joe Aronson [mailto:[log in to unmask]]
Sent: Wednesday, August 18, 1999 7:34 AM
To: [log in to unmask]
Subject: [TN] GALVANIC ETCHING MECHANISM
ALL:
Has anyone out there experimented with etches to see wether a more/less
aggressive etch produces a change in the degree of galvanic etching? It
sounds to me like the main limitation in the mechanism of galvanic etching
is going to be the diffusion of the oxidizer to the more noble metal. Is
this the case?? If there is a known rate determining step please let me
know. I may e able to use it to fight this effect. Thanks.
Joe Aronson
Wet Process Engineer
JMSPI
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
|
|
|