nishath yasmeen wrote:
> We are seeing non uniform plated copper deposits in very small areas on
> silicon wafers from the acid copper plating bath.
>
> I can understand the non uniformity across areas which are large (
> inches) but these areas measure in micron range. The thickness profile
> of this area looks like a staircase on the profilometer. Is this a flow
> problem? Does this depend on the current density?
> What other factors do I need to consider for uniformity improvement?
>
> Any suggestions will be greatly appreciated.
> Thanks,
> Yasmeen
>
> ##############################################################
> TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
> ##############################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
> the body:
> To subscribe: SUBSCRIBE TECHNET <your full name>
> To unsubscribe: SIGNOFF TECHNET
> ##############################################################
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
> information.
> If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
> 847-509-9700 ext.5365
> ##############################################################
Dear Yasmeen:
I would regard your case as pattern plating. In pattern plating, the current densities
on each area vary. Smaller area will take more current and plate more while lager area
will take less current and plate less. I suggest you to use current density of 10
mA/cm**2. If you are plating areas measuring in microns, you need a power supply which
can provide currents in mA for the acid plating bath.
Please correct me if I am wrong!!!!!
Francis
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
|
|
|