Matthew,

Please send me a copy of the aperature shape.      Fax  507-526-3059

Tenison Stone
Telex Communications, Inc.





Matthew Park <[log in to unmask]> on 01/07/98 10:36:30 AM

Please respond to "TechNet Mail Forum." <[log in to unmask]>; Please respond
      to Matthew Park <[log in to unmask]>

To:   [log in to unmask]
cc:    (bcc: Tenison Stone/BlueEarth/Telex)
Subject:  [TN] Stencil Aperture Shapes -Reply




Mr. Windsor:
Post your fax number, so I may fax you a solderpaste
aperture shape that I use for the complete elimination of
solderballs for chip components.  It was proven it works
better than home plate shape.
regards
Matthew Park
>>> Clinton Windsor
<[log in to unmask]> January
7, 1998  1:27 am >>>
Dear Technetters,
We are trying to eliminate the occurence of solder balls in
our
production line by trialling various aperture shapes and
reductions on
the screen printer stencil.  The nature of the solder balls
suggests
that paste is being trapped under the component and then
forms a solder
ball which adheres to the side of the component.  I have seen
this type
of solder ball referred to as a "squeeze ball".  We have tried
the so
called "home plate" (trapezoidal) shaped apertures with
considerable
success on nearly all the components except for the 0603
capacitors.
I would be interested to hear any ideas or suggestions of
other aperture
shapes or designs which could help solve this problem.
Thanks in advance,
Clinton Windsor
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or
847-509-9700 ext.311
##############################################################

##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional information.
For the technical support contact Dmitriy Sklyar at [log in to unmask] or 847-509-9700 ext.311
##############################################################


ATOM RSS1 RSS2