The answer of course is "It Depends".
I agree that 10 minutes is the minimum in most specs. If the ROSE is
being used as a product acceptance metric (not recommended, but done) then
people do not test more than 10 minutes because any more is likely to
result in higher numbers which could lead to product rejection. If the
ROSE is being used for process control, which is what it is supposed to be
used for, if the value continues to climb at 9, 10, 15, 20 minutes, you
have a problem on the board that you need to investigate. You want to go
till you don't see change. If you never get there, then you probably have
a bad solder mask or something else that is chemically breaking down.
Doug Pauls
From: Chris Mahanna <[log in to unmask]>
To: <[log in to unmask]>
Date: 01/26/2012 11:01 AM
Subject: Re: [TN] Typical ROSE Test Duration
Sent by: TechNet <[log in to unmask]>
10 or 15 minutes is very commonly specified.
However, a better answer is: extract what you're interested in, but not
more. If you are starting with the assumption that what you're looking
for is reasonably soluble in 75/25, then the 10 to minutes is likely
appropriate.
What you watch for is asymptotic decrease in extraction rate, and compare
that against your pass/fail threshold.
If you are ANYWHERE near your pass/fail threshold, I highly suggest
reading ILAC-G8.
http://www.ilac.org/documents/ILAC_G8_03_2009.pdf
Chris
Chris Mahanna
Robisan Laboratory
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Garcia, Rigo
(GSFC-300.0)[MANTECH SRS TECHNOLOGIES]
Sent: 2012/01/26 11:16 AM
To: [log in to unmask]
Subject: [TN] Typical ROSE Test Duration
Hi everybody!
I have looked at several document but can't find the answer. This should
be an easy one for my TechNet buddies though.
Does anybody know what the typical duration for the ROSE Test is?
Rigo Garcia
Sr. Quality Assurance Engineer
Workmanship Standards, Code 300
NASA, Goddard Space Flight Center
Greenbelt, MD 20771
Phone. (301) 286-6129
Fax. (301) 286-6576
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts:
send e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives For additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|