Hi Mike - Good information! Do you have any recommended papers/reports on
In based solders I could go read? I don't have much on In based solders in
our knowledge database.
Dave
"Mike Fenner" <[log in to unmask]>
03/11/2010 02:59 AM
Please respond to
[log in to unmask]
To
"'TechNet E-Mail Forum'" <[log in to unmask]>, <[log in to unmask]>
cc
Subject
RE: [TN] Low Temp Solder Paste
Yes, with that alloy combo it is possible that your joints will have an
Sn/In intermetallic zone with MP around 118C and Sn/Pb/In at ~120-130C.
This
could limit the max service temp of those joints to <<100C (depending on
the
number of cycles/mechanical stresses in service etc).
As mentioned by Wayne In can make undesirable intermetallics with Cu, but
presumably this issue was considered when you first determined on the
80In/15Pb/5Ag.
Regards
Mike
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
Sent: Wednesday, March 10, 2010 10:34 PM
To: [log in to unmask]
Subject: Re: [TN] Low Temp Solder Paste
Hi Carl - as Werner described, using a low temperature paste and a
solderball that melts at a higher temperature will result in some type of
metallurgical gradient with different amounts of microstructure/phase
variation dependent on the actual temperature gradient experienced. The
specific solder alloys will play a big role as they determine the types of
phases that will be produced. And with In, Ag, Pb, and Sn in the mix with
the elemental percentages you described, all sorts of "fun" things could
happen. The In/Pb/Ag alloy melts around 150C so you are also going to
have solder joint integrity issues in many high performance use
environments. I would anticipate that the 80% In content makes the paste
cost painful too. Good Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
Carl Ray <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
03/10/2010 04:06 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Carl Ray <[log in to unmask]>
To
[log in to unmask]
cc
Subject
Re: [TN] Low Temp Solder Paste
Sorry about that Werner (I really wanted you to guess :) ). The solder is
80In, 15Pb and 5Ag
________________________________
From: Werner Engelmaier [mailto:[log in to unmask]]
Sent: Wednesday, March 10, 2010 3:44 PM
To: [log in to unmask]; Carl Ray
Subject: Re: [TN] Low Temp Solder Paste
Hi Carl,
You did not say what the paste is.
When you have a high-melt SnPb ball and 63Sn/37Pb paste you wind up with a
good solder joint having a gradient in Sn/Pb concentrations.
When you have a SAC ball and 63Sn/37Pb paste, it depends how long you are
above the Liquidus temperature of the SAC solder and whether you get good
mixing-while it is not the ideal solution alloy, with good mixing the
fatigue resistance is comparable to SAC & SnPb.
In you case-well, IT DEPENDS.
Werner
-----Original Message-----
From: Carl Ray <[log in to unmask]>
To: [log in to unmask]
Sent: Wed, Mar 10, 2010 4:09 pm
Subject: [TN] Low Temp Solder Paste
Hi Technetters!!! I have a question regarding low temp solder paste and
standard
63/37 eutectic BGAs. Has anyone had any experience with this type of
process?
What are the pros and cons? Obviously the BGA doesn't see the temperatures
needed for the balls to collapse so what type of solder joint do you end
up
with?
Carl Ray
Manufacturing Engineering Manager
Teledyne Electronic Manufacturing Services
1425 Higgs Rd.
Lewisburg, TN 37091
Direct: 931-270-2724
Cell: 931-637-5958
Email: [log in to unmask]<mailto:[log in to unmask]
><mailto:[log in to unmask]<mailto:[log in to unmask]>>
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]<
mailto:[log in to unmask]>
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask]<mailto:[log in to unmask]
> with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]<mailto:[log in to unmask]>: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]<mailto:[log in to unmask]>: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for
additional information, or contact Keach Sasamori at [log in to unmask]<
mailto:[log in to unmask]> or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
***This email, its content, and any files transmitted with it, are
intended solely for the addressee(s) and may be legally privileged and/or
confidential. If you are not the intended recipient, please contact the
sender by return and delete the material from any computer. Any review,
retransmission, dissemination, or other use of, or taking of any action in
reliance upon this information by persons or entities other than the
intended recipient is prohibited.
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|