I don't know what kind of improvements have been made in the last five
years. I'm sure there have been some.
We evaluated various finishes between 2000 and 2003.
We discovered that all Imm Sn coatings were not the same.
In addition to thickness there is an organic additive to protect the tin.
If there is a failure of this organic the tin does not perform well after
thermal cycle.
In some cases not as well as a bare copper control sample.
I am not a metallurgist but I understand the fluxes we use are designed to
reduce copper oxides and that tin oxides are more difficult to reduce.
Which might explain why a failure of the coating can be worse than no
coating.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Peter Barton
Sent: Tuesday, September 22, 2009 12:33 PM
To: [log in to unmask]
Subject: [TN] Imm Sn soldering issue.
Dear Technetters,
Hopefully there is someone out there who can help me understand a very
specific issue we have using PCB's plated with Imm Sn. namely, non-wetting
of solder to some lands on the second side of population after reflow. We
have an understanding of this surface finish with respect to the assembly
processes. We are careful how we handle the unpopulated PCB's, the PCB's are
shipped directly to the line and are only removed from the manufacturer's
packaging at the point of use. They are not pre-baked and are subjected to 2
relatively benign reflow cycles.
We only ever see the issue on the second side. It occurs on various
component types. When it does occur the solder deposited at the printing
stage is reflowed and is attached to the component termination, favouring
this as more wettable than the PCB land. The problem does not always occur.
The assembly is populated in 2 up panels and we have examples where one
panel has soldered joints across the piece, whilst the other PCB in the same
panel exhibits non wetting in some areas.
The assembly has been profiled with a good distribution of thermocouples on
a sample assembly to confirm a low delta T and the profile itself is right
at the centre of the paste manufacturer's recommendations. We like to have a
good process window.
I am aware that the 2 possible reasons for this condition are (a) thermal
degradation of the finish and (b) possible plating quality issues.
We have dismissed excessive thermal input as these have only been subjected
to 2 non-RoHS thermal cycles and the PCB's are fresh from the manufacturer.
Peak temperatures are only around the 227 deg. C mark. The Sn thickness
specification is 0.8 - 1.2 uM. The applied thickness has been measured using
XRF as a process control and averages 1.0 uM. I am aware that XRF is only a
guide as it cannot segregate out 'available' pure Sn from Sn/Cu
intermetallics.
We have had an independent lab analysis conducted and example lands where
this condition is seen are shown to have very little or no remaining Sn at
the surface, the majority being Sn/Cu intermetallics. Other unpopulated
plated areas have also been subjected to SEM and EDX for comparison and
exhibit what is described as 'islands' of Sn in a sea of Cu/Sn
intermetallics.
We have not had 'virgin' PCB's analysed yet for comparison as it is costly
and we are not sure if we would pick the correct example to look at - it
could be a good one.
For the PCB experts out there out there I have a couple of questions:
1. If the application of Sn is a displacement reaction with the underlying
Cu is there any way that there can be less Sn on some surface areas than
others?
2. Are there other reasons that there could be variation in Sn deposits or
could lead to the 'islands' of Sn as described by our lab that is seen after
thermal processing?
3. Are we missing anything else?
Any questions please feel free to ask - this is causing me the biggest
headache going.
Peter Barton
Senior Process Engineer
ACW Technology Ltd
Dinas Isaf West
Tonypandy
Mid Glamorgan
CF40 1XX
Tel: 01443 425275 (direct)
Fax 02380 484882
[log in to unmask]
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|