We have seen this a few times. There seem to be two reasons why: CTE
mismatch Cu/Ni and brittle Nickel caused by excessive additives.
Inge
----- Original Message -----
From: "Lee Whiteman" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Wednesday, February 11, 2009 7:20 PM
Subject: [TN] CRACKED ENIG PADS
I have asked Steve to put up a pair of pictures I received. They are of
cracks within the ENIG finish of a PWB. I know that the board failed,
based on IPC-6011 and IPC-6012.
My question is what would cause the cracking? Evidently, it is in the
Nickel layer and the copper layer was not compromised. There was no
evidence of a lack of bonding between the copper and the ENIG finish.
These boards are fresh from the supplier.
Just curious...
Thanks in advance.
Lee Whiteman, PMP
Senior Member Engineering Staff
L-3 Communications East
Telephone: (856) 338-3508
FAX: (856) 338-2906
E-Mail: [log in to unmask]
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|