Ido,
Have U checked the copper plating ....tensile/elongation & purity.
If it is acid copper...for a well maintained bath, elongation should be above 20%.
Rashesh
Accurate Engg Inc
www.accueng.com
-----Original Message-----
From: Whittaker, Dewey (EHCOE) <[log in to unmask]>
To: [log in to unmask]
Sent: Tue, 7 Oct 2008 7:02 am
Subject: Re: [TN] Barrel and Corner cracks in copper elctroplating
You know me too well. My hands were on the keyboard when your message
popped up. I have been traveling on business for three weeks and didn't
want to lose the touch.
Dewey
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D.
Sent: Tuesday, October 07, 2008 5:41 AM
To: [log in to unmask]
Subject: Re: [TN] Barrel and Corner cracks in copper elctroplating
Don't go there Dewey.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Igoshev, Vladimir
Sent: Tuesday, October 07, 2008 7:37 AM
To: [log in to unmask]
Subject: Re: [TN] Barrel and Corner cracks in copper elctroplating
Well, Cu can be very ductle, but whether necking wil occur or not
depends on a lot of things. In case of barrel cracks it can become even
more complicated as the quality of plating can make it look as necking.
Regards,
Vladimir
----- Original Message -----
From: TechNet <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Sent: Tue Oct 07 08:27:57 2008
Subject: Re: [TN] Barrel and Corner cracks in copper elctroplating
Oh yes I find the copper is plastically deformed and it appears that is
happening here. Look for a thinning right at the break site. With fast
onset catastrophic type failures thinning is frequently observed. Copper
thinning is s very subtle condition however and is usually over looked.
You know there is a lot more to be said about barrel cracks, crack
propagation, roots causes etc. and not enough time to do so in this
forum. I just try to hit the major points.
Sincerely,
Paul Reid
Program Coordinator
PWB Interconnect Solutions Inc.
235 Stafford Rd., West, Unit 103
Nepean, Ontario
Canada, K2H 9C1
613 596 4244 ext. 229
Skype paul_reid_pwb
[log in to unmask] <mailto:[log in to unmask]>
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier /*
Sent: Tuesday, October 07, 2008 4:43 AM
To: [log in to unmask]
Subject: Re: [TN] Barrel and Corner cracks in copper elctroplating
Hi Paul,
Inward bowing of the barrel walls certainly occurs. However, in order to
cause cracks like these, the copper would have to plastically deform and
stay bowed. I did not see this.
WernerNew MapQuest Local shows what's happening at your destination.
Dining, Movies, Events, News & more. Try it out!
(http://local.mapquest.com/?ncid=emlcntnew00000001)
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|