To Bogert:
You need to see a profile of the pwb from your OEM, not just the machine
settings. Insist on this. Once you have this, post another technet with
profile/pwb information (max component and circuit side temperature,
solder contact (dwell) time.
As for the machine settings, 350C is typical of the preheat setting used
on the Soltec machine with VOC fluxes. And 260C (500F) is used widely
throughout the industry. I question the .9ft/min. This all depends on
the width of the wave and the solder dwell time. The slowest I've ever
run on the Soltec (with a .250" backplane) was 2.0 ft/min (which gave me
about a 6 second dwell time).
Al
- bogert <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
10/04/2008 07:37 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
- bogert <[log in to unmask]>
To
[log in to unmask]
cc
Subject
[TN] Wave soldering temperature profile question
October 3, 2008
We have an OEM that is wave soldering a 0.125 inch thick backplane
assembly.
The assembly contains just press-fit VME connectors (added after wave
soldering) and some PTH and SMT passive parts (capacitors and resistor
networks). The SMT parts are hand soldered. Board material is
IPC-4101/21,
24, 26.
The OEM wave soldering machine settings are one single bottom preheater
set
at 350C with solder pot set at 260C. Conveyor speed is 0.9 feet/minute.
Solder is Kester Sn63pb37; flux is Kester 971M; flux applied by foam
method.
Solder machine is older Soltec Model 6551.
My question is; for this specific application, what is the recommended
maximum preheat temperature? Seems to me that 350C is too high. Is this
high a temperature compatible with the Tg of the FR4 board material? Is
there any concern with damaging the board material from overheating?
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|