TECHNET Archives

October 2008

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
[log in to unmask], TechNet E-Mail Forum <[log in to unmask]>
Date:
Tue, 28 Oct 2008 11:59:50 +0800
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Tan Geok Ang <[log in to unmask]>
Subject:
From:
Tan Geok Ang <[log in to unmask]>
Content-Transfer-Encoding:
7bit
In-Reply-To:
Content-Type:
text/plain; charset="iso-2022-jp"
MIME-Version:
1.0
Parts/Attachments:
text/plain (48 lines)
Hi Werner,

                        Thank for the link. Good write out!

 

Regards

GA Tan

________________________________

From: [log in to unmask] [mailto:[log in to unmask]] 
Sent: Monday, 27 October 2008 2:06 AM
To: Tan Geok Ang; [log in to unmask]; [log in to unmask]
Subject: Re: [TN] Underfill, Cause

 

Nee hao GA Tan,
The Tg of the underfill is not much of a concern; the critical properties are the CTE over the application T-range and the modulus of elasticity. It has also been shown by work done at Motorola that slow curing underfills [at least some] do not give much reliability improvement at low failure probabilies [that is the failure distributions become very wide]; whereas snap-cure underfills produce tight failure distributions.
You might want to take a look at my reliability column: Engelmaier, W., “Reliability Improvement with Underfill,” Global SMT & Packaging, Vol. 6, No. 3, March 2006, pp. 66-67. 

Regards,
Werner Engelmaier
可靠性先生
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Cell: 386-316-5904
E-mail: [log in to unmask], Website: www.engelmaier.com


**************
Play online games for FREE at Games.com! All of your favorites, no registration required and great graphics check it out! (http://pr.atwola.com/promoclk/100000075x1211202682x1200689022/aol?redir= http://www.games.com?ncid=emlcntusgame00000001)


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2