It is possible to solder SAC balls using Pb:Sn solder. BUT...
It is important that the profile be adjusted so the SAC balls fully melt
and there is enough time for the two types of solder to mix well,
preventing the stratification of solders often noted when this is tried.
I know of no way to check for this full mixing except through cross
sectioning polishing and either looking for PB islands in all parts of
the solder ball, and verifying by EDX that Pb is found throughout the
solder ball. You need to be able to view the Pb islands in order to
exclude the possibility of Pb smearing over the surface when polishing.
mark
Mark Woolley
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Croslin, Robert
Sent: Tuesday, October 21, 2008 10:10 AM
To: [log in to unmask]
Subject: Re: [TN] Lead Free BGA'S
We had one of our long time CM's do exactly this on a project last year
with disastrous results. They did it without our knowledge trying to
meet an impossible schedule. Some of the devices passed test and began
failing immediately while others never passed. They had to rebuild the
entire lot on their nickel. The only positive thing was when one of our
other proposed doing the same thing recently and we were able to say
H**L NO! Like Deac replied "It's either lead free or it AIN'T!!!!!!!!!"
Bob Croslin
The Nielsen Company
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of John Foster
Sent: Tuesday, October 21, 2008 11:21 AM
To: [log in to unmask]
Subject: [TN] Lead Free BGA'S
Our assembly house recently assembled some boards with Lead Free BGA's
for us and when I asked them if they used a lead free process they
responded with.
We use leaded solder (Sn63Pb37) with a hybrid oven profile to
accommodate the lead-free BGA. I hope this answers your question. Please
let me know if you have any more questions."
Is this a common process, is this a reliable process
Any input is appreciated
Thank You
John Foster
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|