My intuitive opinion is that 1 out of 64 is no problem, especially for
consumer grade, likely 5 year or less lifetime. However, if the app.
actually stresses the BGA to its limits with all 64 spheres, and you
remove one, then a more careful analysis is necessary. Since the most
stress is at the corner positions, the analysis of the stress
distribution with the corner ball removed might actually REDUCE stress
on the remaining balls.
Usually the predominant stress is thermal cycling combined with the
creep due to stress relaxation after the post-reflow cooldown. But
there are other possibilities: Is it possible to flex the circuit the
BGA is attached to during the usage life? I have trouble imagining any
consumer app where the mass of the BGA would come into play, unless this
app involves projectiles.
Wayne Thayer
>>> [log in to unmask] 11/17/2006 12:50:56 pm >>>
Bob,
As long as the laminate isn't cracked under other pads (as a result of
the board handling/service), then it should be OK if you "glue down"
just one pad.
Vladimir
-----Original Message-----
From: TechNet
To: [log in to unmask]
Sent: Fri Nov 17 12:37:06 2006
Subject: Re: [TN] One solder Ball Not Connected on a No Connect Pad
After Rework
All:
Thanks for your responses. One of the weaknesses of this forum is
the lack of ability to load photos and movies into the thread to
explain the case with pictures whihc are worth much more than words in
these cases.
Perhaps I should explain the repair more thoroughly.
We are suggesting to this customer (Class II, consumer grade product)
that we "cut off" the pad and epoxy down any remnant pad. This is much
less expensive Amercian labor than doing a complete IPC 7721 repair.
The real issue that I am asking for input from the esteemed group on
is the pull strength.....
Thanks
Bob
"Stadem, Richard D." <[log in to unmask]> wrote: When the pad
is lifted, it typically exposes the fiberglass weave
underneath the pad. This allows moisture, flux, solvents, etc, to
enter
the pwb and can cause problems later.
The answer to your question depends on what the assembly is used for,
and to what standard do you wish to comply with. IPC 610 and J-STD-001
do not allow missing pads, they require it be repaired.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of bob wettermann
Sent: Friday, November 17, 2006 9:11 AM
To: [log in to unmask]
Subject: [TN] One solder Ball Not Connected on a No Connect Pad After
Rework
This question to the group is about expected solder joint strength on
a
BGA.
The BGA in question is a 8 x 8mm plastic package BGA using a LF
SAC305 soldering process. It has 64 x 0.018" balls holding it to the
PCB.
When removing this device for rework 3-4% of the time one of the
corner NO CONNECT pads comes off.
The question is if we do nothing upon replacement of a new device
to
the damaged pad will it really make a difference ??? We are arguing
that the holding strength of the reworked device would be
approximately
the same because the change in overall surface area is marginally
impacted.
Thanks
Bob Wettermann
Bob Wettermann
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
PH 847-767-5745
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
Bob Wettermann
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
PH 847-767-5745
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|