Arnaud,
I don't know if the package materials are different, Practical Components don't supply this information.
The thermal profile was derived from studies I've read so therefore you could call it a hybrid one..
Having seen the packages that are required for production they are somewhat different than the dummy ones, I was trying to get a flyer on this larger package which we haven't assembled yet in production.
-----Original Message-----
From: [log in to unmask]
[mailto:[log in to unmask]]
Sent: 16 November 2006 11:33
To: TechNet E-Mail Forum; Braddock, Iain
Subject: Re: [TN] BGA anomaly
*** WARNING ***
This mail has originated outside your organization,
either from an external partner or the Global Internet.
Keep this in mind if you answer this message.
Hello Iain,
Story sounds familiar here, although not so catastrophic...
BGA material change might be the explanation: lead-free BGAs are
designed to withstand hotter reflow profiles and use more thermally
resistant materials like molding compounds and die attach glue. This has
a direct impact on the warpage orientation and value.
Note also that your specific daisy-chained component has a small die
size compared to the BGA dimensions, which is un favourable in terms of
warpage (check with X-Ray).
Question: Was your refow profile a SnPb, SAC or an hybrid one?
Hope this helps.
A. Grivon
Braddock, Iain a écrit :
> Techies, need a little help here!
>
> In preparation for assembling some development boards with an 1152 PBGA, I purchased some Practical Components dummy boards & devices double sided ENIG and 1156 PBGA'. I took the opportunity to get 63/37SnPb and leadfree (SAC 305) BGA's which are identical in sized. Alloy comfirmed by XRF.
>
> The evaluation boards (PCB012) amongst others had footprints for 2 off 1156 devices, so populated 1 off each component per board.
>
> I asked TSL (UK) to provide a stencil with their recommendations and ended up with a 0.005" S/S laser cut with 0.0005" aperture reduction.
>
> The paste used was our standard multicore 62/36/2 SnPbAg
>
> The reflow profile peaked @ 232C with time above liquidus for, 1) SAC - 29 secs 2) SnPb - 74 secs.
>
> Now comes the fun bit:
>
> Post reflow the SAC BGA had a stand off of 0.4mm in the centre (sides) but less in the corners ie. curled down, and all 4 corners with solder bridges.
> The 63/37 BGA had a stand off of ~ 0.5mm but this time at the 4 corners with slightly less in the middle (I crudely used feeler gauges!)
>
> So it would appear that one BGA curled up and the other curled down....with different amounts of collapse.........hmm?
>
> Anyone provide an explanation of this phenomenon?
>
> CIA,
> Iain.
>
>
>
> ********************************************************************
> This email and any attachments are confidential to the intended
> recipient and may also be privileged. If you are not the intended
> recipient please delete it from your system and notify the sender.
> You should not copy it or use it for any purpose nor disclose or
> distribute its contents to any other person.
> ********************************************************************
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>
********************************************************************
This email and any attachments are confidential to the intended
recipient and may also be privileged. If you are not the intended
recipient please delete it from your system and notify the sender.
You should not copy it or use it for any purpose nor disclose or
distribute its contents to any other person.
********************************************************************
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|