TECHNET Archives

September 2006

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Stadem, Richard D." <[log in to unmask]>
Date:
Thu, 21 Sep 2006 14:36:03 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Lee parker <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
7bit
Content-Type:
text/plain; charset="iso-8859-1"
From:
Lee parker <[log in to unmask]>
Parts/Attachments:
text/plain (120 lines)
Rich is right.

Just think of the outcome if RoHS had been imposed on Mr. Lincoln's Yankee
Army.




----- Original Message -----
From: "Stadem, Richard D." <[log in to unmask]>
To: <[log in to unmask]>
Sent: Thursday, September 21, 2006 2:30 PM
Subject: Re: [TN] Dissolving copper hole wall using lead free HASL?


But Dewey, you don't need to worry about it or gather all that data.
Remember what DDave from NY said last week? He said that us
old-fashioned military supplier dweebs should not be opposed to using
Pb-free processes and materials, that they were just as reliable as
existing qualified processes. So c'mon, Dewey, get with it. Don't be an
old stick-in-the-mud. Something like this does not need qualification.
Just throw it out there. DDave said it would work. So what if the hole
wall might wash away from the SAC alloy? Is no big deal, eh? What else
don't we know?..... I can't wait to start build some flight control
modules for spacecraft with SAC plating on the board, and with 99% tin
finish on the component leads AND with 99% tin in the solder paste AND
with new pwb materials specially formulated to withstand blowtorch
soldering AND....darn, my keyboard just quit working. It must have
something to do with this green sticker on it.

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Whittaker, Dewey
(EHCOE)
Sent: Thursday, September 21, 2006 11:57 AM
To: [log in to unmask]
Subject: Re: [TN] Dissolving copper hole wall using lead free HASL?

That's correct. We are gathering a lot of data to support the premise
that SAC soldering of Copper PTHs is a no-no.
Dewey

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Dennis Fritz
Sent: Thursday, September 21, 2006 9:49 AM
To: [log in to unmask]
Subject: Re: [TN] Dissolving copper hole wall using lead free HASL?

Well, it stripped out the "cut and paste" from the pdf of Jasbir's slide
at IPC.  Here is what he said on the slide:


During rework with SnAgCu alloy with copper from the PCB: copper
dissolves with increasing contact time.

Experience: PTH barrel knee erosion after  20 seconds of solder pot
dwell time

Copper dissolution is a function of  original barrel/pad thickness,
solder temperature and alloy (tin percentage),  dwell/contact time and
solder flow rate and type of copper plating.

Studies are ongoing with dissolution rate comparison with various
lead-free solder alloys and process optimization.


Denny Fritz

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2