TECHNET Archives

September 2006

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Stadem, Richard D." <[log in to unmask]>
Date:
Tue, 12 Sep 2006 13:13:46 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Lee parker <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
7bit
Content-Type:
text/plain; charset="iso-8859-1"
From:
Lee parker <[log in to unmask]>
Parts/Attachments:
text/plain (123 lines)
Helena

Richard has covered most of the issues associated with delaination. I would
add another, reduced dielectric electrical strength which can cause internal
arcing. As some of us learned the hard way this can stimulate a new career.

Best regards

Lee

J. Lee Parker, Ph.D.
JLP Consultants LLC
804 779 3389


----- Original Message -----
From: "Stadem, Richard D." <[log in to unmask]>
To: <[log in to unmask]>
Sent: Tuesday, September 12, 2006 1:02 PM
Subject: Re: [TN] Delamination


Good question, Helena.

Three major reasons why delamination of the substrate is "bad" (read:
cause reliability issues) that come to mind quickly:

1. Delamination puts tremendous pressure on the z-axis of the via wall,
and will lead to separation (electrical open) between the top and bottom
portions of the via hole wall. This would leave the top layer
disconnected from the bottom layer of that particular network, or would
disconnect inner layer traces from the source via. Trace pullaway from
the via will also cause the circuit to fail.

2. Delamination puts extreme stresses on the solder joints. Flexing the
pwb material upwards from any points anchored to vias and through-hole
connections puts stress on the solder, leading to pre-mature failure due
to cracking and creep-fatigue-related solder joint failures. The void
will expand and contract with temperature cycles.

3. Delamination creates a resin void. Actually, it is the other way
around, in that delaminations are usually caused by an abcess that
begins as a resin void. In any case, an air pocket is left inside the
pwb. This can continue to expand if the assembly is thermally cycled
during its normal operation in the field, further damaging the surface
foil and via substrates that are in the area of the delamination.

4. Condensation and flux entrapment can form in the delamination,
causing electrical performance issues.

5. Delamination on high-frequency/high-impedance will disturb the
impedance of the net. This has to be carefully controlled.

6. Dielictric properties of the pwb will change and become unstable.

And lots and lots of other reasons.


-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Pasquito, Helena
Sent: Tuesday, September 12, 2006 11:45 AM
To: [log in to unmask]
Subject: [TN] Delamination

Hi TechNetters,

Let me ask a question; I know delamination is bad, but why?  What is the
failure mode to the board when a board delaminates and would there ever
be an instance that a board that delaminates is still OK to use?  This
is a Class 3 application.  Yes, I know what the IPC standards say but
not real sure about the board process.  Yes, I "googled" and there is a
lot of stuff out there.  Maybe someone can recommend some reading
material (hopefully short and sweet and to the point).

Thanks!
Helena

Helena Pasquito
Manufacturing Skills Instructor
M/A-COM, Tyco Electronics
1011 Pawtucket Blvd., M/S 107
Lowell, MA 01853
978-442-5024
[log in to unmask]


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2