The material Tg specifications are only part of the overall formula.
Just because a laminate is classified with a Tg of 170 does not mean
that the high-Tg material was manufactured using quality materials and
laminated together properly. Board vendors buy their laminates from
laminate vendors. The Tg means nothing if it is not laminated together
with a good resin epoxy, etc, etc. A material with excellent Tg (and
even Td) properties can still delaminate at temperatures as little as
210 C, even when pre-baked to remove moisture. The Z-axis expansion
factor, the Td factor, and many other material properties play a part.
-----Original Message-----
From: Leadfree [mailto:[log in to unmask]] On Behalf Of Phil Nutting
Sent: Tuesday, May 09, 2006 1:25 PM
To: [log in to unmask]
Subject: Re: [LF] Cost pressures starting!
Ioan,
You are making me nervous. We have switched to specifying Isola 410
with a 170Tg in stiff 0.062" configuration. Are you suggesting it will
delaminate? Yikes! I ran some tests with Isola 402 trying to blister
them, but they took the beating.
Phil
-----Original Message-----
From: Leadfree [mailto:[log in to unmask]] On Behalf Of Tempea, Ioan
Sent: Tuesday, May 09, 2006 12:37 PM
To: [log in to unmask]
Subject: Re: [LF] Cost pressures starting!
Pete,
our first attempt to run lead-free was on a PCB with 170Tg, because we
assumed at that time this would take care of the temperautre raise.
Guess what? We ended up with the most extensive delamination I have ever
seen. And it was a consumer good, 6 layer, lightly populated assembly.
So, if you are lucky and you see delam after the first pass, you will
scrap all the boards in stock, because if it happens it happens on all
the PCBs from that batch. Add the cost of the scrapped material to the
cost of losing the contract because you cannot deliver.
Then, if you are almost lucky, you will see delam after more thermal
excursions. This means that you scrap more material and you cope again
with compromised delivery schedule.
And if you are not lucky, you won't see a thing, you test OK, you ship
and the products die in the field right after that, due to latent damage
to the PCB structure.
Ask your bean counters to make a paradigm shift: they should make sure
that more is charged to the customer. There is no other way.
Regards,
Ioan
-----Original Message-----
From: Leadfree [mailto:[log in to unmask]]On Behalf Of Lee parker
Sent: Tuesday, May 09, 2006 11:02 AM
To: [log in to unmask]
Subject: Re: [LF] Cost pressures starting!
Pete
The variable that the accounts always overlook in cases such as this is
the yield impact. If you continue using 140 Tg materials you will
undoubtedly decrease the yield of your assembly process not to mention
increased customer returns.
You can understand the trade offs by first calculating the cost of a
unit degradation in yield. Then determine how much yield impairment you
can tolerate as a result of continuing to use the present materials in a
more aggressive assembly environment. I imagine any reasonable estimate
in the yield impairment will show an advantage for using the more
expensive high performance materials.
Best regards
Lee
J. Lee Parker, Ph.D.
JLP Consultants LLC
804 779 3389
----- Original Message -----
From: "Pete Houwen" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Tuesday, May 09, 2006 10:11 AM
Subject: [LF] Cost pressures starting!
> We have successfullly made the transtition, and are beginning to
produce
> complaint products.
>
> And that's starting to drive the bean counters into a frenzy. Our new
PCB
> material spec is calling for 330Td, non-dicy, Z-Axis max, etc... and
guess
> what, - it costs more than the old 140Tg material. Now they want to
go
> back to the old material - throw out a year of research and testing -
> because they ran a few boards using the old material.
>
> The questions are - is anyone running lead free solder processes using
the
> old standard 140Tg, in any kind of volume, with any measurable
quality?
>
> How do you convince them that RoHS just costs more, but it will get
> cheaper eventually?
>
>
------------------------------------------------------------------------
-------Leadfee
> Mail List provided as a service by IPC using LISTSERV 1.8d To
> unsubscribe, send a message to [log in to unmask] with following text
in
> the BODY (NOT the subject field): SIGNOFF Leadfree To temporarily
> stop/(start) delivery of Leadree for vacation breaks
send:
> SET Leadfree NOMAIL/(MAIL)
> Search previous postings at: http://listserv.ipc.org/archives Please
> visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at
[log in to unmask] or
> 847-615-7100 ext.2815
>
------------------------------------------------------------------------
-------
>
------------------------------------------------------------------------
-------Leadfee Mail List provided as a service by IPC using LISTSERV
1.8d To unsubscribe, send a message to [log in to unmask] with following
text in the BODY (NOT the subject field): SIGNOFF Leadfree To
temporarily stop/(start) delivery of Leadree for vacation breaks
send: SET Leadfree NOMAIL/(MAIL)
Search previous postings at: http://listserv.ipc.org/archives Please
visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
------------------------------------------------------------------------
-------
------------------------------------------------------------------------
-------Leadfee Mail List provided as a service by IPC using LISTSERV
1.8d To unsubscribe, send a message to [log in to unmask] with following
text in the BODY (NOT the subject field): SIGNOFF Leadfree To
temporarily stop/(start) delivery of Leadree for vacation breaks
send: SET Leadfree NOMAIL/(MAIL)
Search previous postings at: http://listserv.ipc.org/archives Please
visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
------------------------------------------------------------------------
-------
------------------------------------------------------------------------
-------Leadfee Mail List provided as a service by IPC using LISTSERV
1.8d To unsubscribe, send a message to [log in to unmask] with following
text in the BODY (NOT the subject field): SIGNOFF Leadfree To
temporarily stop/(start) delivery of Leadree for vacation breaks send:
SET Leadfree NOMAIL/(MAIL) Search previous postings at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
------------------------------------------------------------------------
-------
-------------------------------------------------------------------------------Leadfee Mail List provided as a service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Leadfree
To temporarily stop/(start) delivery of Leadree for vacation breaks send: SET Leadfree NOMAIL/(MAIL)
Search previous postings at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-------------------------------------------------------------------------------
|